Stainless acid-resistant steel 1.4429, X2CrNiMoN17-13-3, 1.4406, X2CrNiMoN17-11-2, AISI 316LN, UNS S31653 according to EN 10088-1.

 

Norma Gatunek Stali
Skład Chemiczny %
C: Mn: Si: P: S: Cr: Mo: Ni: N:
EN 1.4429 - X2CrNiMoN17-13-3
<0.03 <2.0 <1.0 <0.045 <0.030 16.5 - 18.5 2.5 - 3.0 11.0 - 14.0 0.12 - 0.22
EN 1.4406 - X2CrNiMoN17-11-2
<0.03 <2.0 <1.0 <0.045 <0.030 16.5 - 18.5 2.0 - 2.5 10.0 - 12.5 0.12 - 0.22
ASTM UNS S31653 - AISI 316LN
<0.03 <2.0 <1.0 <0.045 <0.030 16.0 - 18.0 2.0 - 3.0 10.0 - 14.0 0.10 - 0.16
BS 316S63 - 316 S 63
<0.03 <2.0 <1.0 <0.045 <0.030 16.5 - 18.5 2.5 - 3.0 11.5 - 14.5 0.12 - 0.22
NF Z3CND17-12Az - Z 3 CND 17-12 Az
<0.03 <2.0 <0.75 <0.040 <0.015 16.0 - 18.0 2.5 - 3.0 11.0 - 13.0 0.12 - 0.20

 

1.4429, 1.4406, AISI 316LN - specification and application

Austenitic acid-resistant steel resistant to intergranular and crevice corrosion with increased content of Nitrogen and Molybdenum. From standard grades of group 316 it is distinguished by significantly better resistance to chlorides, sea water, acids, cracks and product fatigue during work. In addition, the improved chemical composition allows the material to be used at elevated temperatures in much more aggressive environments than standard 316 steel.

It is used in the production of pump parts, installations and pipelines, parts of radiators, special tanks, heat exchangers, agitators, surgical instruments, prostheses, machine components in the pharmaceutical, chemical, petrochemical, cryogenic, cellulose and food processing industries.


Mechanical properties of 1.4429, X2CrNiMoN17-13-3, AISI 316LN

  • Tensile strength, Rm: 580 - 800 MPa
  • The yield point, Rp0,2: >280 MPa
  • Elongation, A:> 40%
  • Modulus of elasticity, E: 220 GPa
  • Hardness, HB: <250
  • Specific resistance, Ω: 0.75 mkOhm * m
  • Impact resistance, KV: > 60J
  • Linear expansion coefficient, α: 16.0 * 10-6 K-1
  • Thermal conductivity, λ: 15.0 W * m-1 * K-1
  • Thermal capacity, cp: 500 J * kg-1 * K-1

 


Mechanical properties at elevated temperatures

Temperature (℃) 100 150 200 250 300 350 400 450 500 550
The yield point, Rp0,2 (MPa) >211 >185 >167 >155 >145 >140 >135 >131 >129 >127
Linear expansion coefficient, α (* 10-6 K-1) 16.0 - 16.5 - 17.0 - 17.5 - 18.0 -
Modulus of elasticity, E (GPa) 194 - 186 - 179 - 172 - 165 -

 


Heat treatment

  • Supersaturation at 1030 - 1110 ℃ with cooling in water or air

 


In the above mentioned grades we supply:

 


Other grades designations:

X2CrNiMoN17133E, X 2 CrNiMoN 17-13-3, AISI 316 LN, DMV 316 LN, 8MLN, 316S63, 316 S 63, Z3CND17-12Az, Z 3 CND 17-12 Az, 1.4495, UNS S31653, 1.4406, X2CrNiMoN17-11-2.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.