Stainless acid resistant steel 1.4439, AISI 317LMN, UNS S31726 with austenitic structure resistant to intergranular corrosion according to EN 10088-1.

 

StandardsSteel Grades
Chemical Composition %
C:Mn:Si:P:S:Cr:Ni:Mo:N:
EN1.4439 - X2CrNiMoN17-13-5 - X 2 CrNiMoN 17-13-5
<0.03<2.0<1.0<0.045<0.01516.5 - 18.512.5 - 14.54.0 - 5.00.12 - 0.22
EN1.4434 - X2CrNiMoN18-12-4 - X 2 CrNiMoN 18-12-4
<0.03<2.0<1.0<0.045<0.01516.5 - 19.510.5 - 15.03.0 - 4.00.1 - 0.2
ASTMUNS S31726 - AISI 317LMN
<0.03<2.0<1.0<0.045<0.03017.0 - 20.013.5 - 17.54.0 - 5.00.1 - 0.2
AFNORZ3CND18-14-05Az - Z 3 CND 18-14-05 Az
<0.03<2.0<0.75<0.035<0.01017.0 - 19.013.0 - 15.04.0 - 5.00.12 - 0.20

 

1.4439, X2CrNiMoN17-13-5, AISI 317LMN - specification and destination

Type 1.4439 is a derivative and better austenitic variant of the 316 and 317 steel grades, having higher Nickel, Molybdenum and Nitrogen content, which significantly increases the product's resistance to pitting and crevice corrosion in Cl environments.

Stal finds its application in the chemical, energy, cryogenic, petrochemical, pulp and paper industries as well as in food contact with chlorides and the effects of high temperatures.

It shows a better yield point up to 400 ℃ compared to 1.4438, 1.4436, 1.4435 and 1.4432.

It is used for the production of special pumps, installations, radiators, apparatus, heat exchangers or tanks for chemicals - sulfuric, formic, nitric, acetic or sodium hydroxide in the form of bars, forgings, sheets and pipes.

The process of heat treatment - supersaturation is carried out at 1020 - 1120 ℃


Mechanical and physical properties of 1.4439, X2CrNiMoN17-13-5:

  • Tensile strength, Rm: 580 - 800 MPa
  • Yield point, Rp0,2: >280 MPa
  • Elongation, A: >35%
  • Impact resistance, KV20℃: >100 J
  • Hardness: <250 HB
  • Heat conductivity, λ: 14 W * m-1 * K-1
  • Heat capacity, cp20℃: 500 J * kg-1 * K-1
  • Modulus of elasticity, E: 200 GPa
  • Specific resistance, Ω: 0.85 mkOhm * m

 


Mechanical properties at elevated temperatures

  • Yield point, Rp0,2
    • temp. 100℃ = >225 MPa
    • temp. 200℃ = >185 MPa
    • temp. 300℃ = >165 MPa
    • temp. 400℃ = >150 MPa
  • Linear Expansion Factor, α
    • temp. 100℃ = 16,0 x 10-6 K-1
    • temp. 200℃ = 16,5 x 10-6 K-1
    • temp. 300℃ = 17,0 x 10-6 K-1
    • temp. 400℃ = 17,5 x 10-6 K-1
    • temp. 500℃ = 18,0 x 10-6 K-1
  • Modulus of elasticity, E
    • temp. 100℃ = 194 GPa
    • temp. 200℃ = 186 GPa
    • temp. 300℃ = 179 GPa
    • temp. 400℃ = 172 GPa
    • temp. 500℃ = 165 GPa

 


In the aforementioned grades we offer:

 


Other alternatives and indications of 1.4439 grade:

X2CrNiMoN 17135, X2CrNiMoN17-13-5, 022Cr19Ni16Mo5N, 1.4434, X2CrNiMoN18-12-4, X 2 CrNiMoN 18-12-4, CLC 17-13-5LN, AISI 317LMN, 17-14-4LN, S31726, S31725, S31753, TP317LMN.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.