Stainless acid-resistant steel 1.4438, X2CrNiMo18-15-4, AISI 317L according to EN 10088-1.

 

StandardSteel Grade
Chemical Composition %
C:Mn:Si:P:S:Cr:Ni:Mo:N:
EN1.4438 - X2CrNiMo18-15-4
<0.030<2.0<1.0<0.045<0.03017.5 - 19.513.0 - 17.03.0 - 4.0<0.11
ASTMAISI 317L - UNS S31703
<0.035<2.0<1.0<0.045<0.03018.0 - 20.011.0 - 15.03.0 - 4.0-
NFZ3CND19-15-04
<0.03<2.0<0.75<0.035<0.01017.5 - 19.514.0 - 16.03.0 - 4.0-
BS317S12
<0.03<2.0<1.0<0.045<0.03017.5 - 19.514.0 - 17.03.0 - 4.0-

 

1.4438, X2CrNiMo18-15-4, AISI 317L - specification and application

Austenitic acid-resistant special steel, used in the production of heat exchangers, pipelines, fittings, parts of radiators and pumps, connectors, tanks for chemical compounds, bolts and nuts. It is mainly used in the chemical, petrochemical, nitrogen, food, refinery, cryogenic and paper industries. Steel resistant to intergranular corrosion.


Mechanical properties of 1.4438, AISI 317L

  • Tensile strength, Rm: 500 - 700 MPa
  • The yield point, Rp0,2: >200 MPa
  • Elongation, A:> 40%
  • Modulus of elasticity, E: 200 GPa
  • Hardness, HB: <215
  • Specific resistance, Ω: 0.85 mkOhm * m
  • Impact resistance, KV: > 60J
  • Linear expansion coefficient, α: 16.0 * 10-6 K-1
  • Thermal conductivity, λ: 14.0 W * m-1 * K-1
  • Thermal capacity, cp: 500 J * kg-1 * K-1

 

Temperature (℃)100150200250300350400450500550
Modulus of elasticity, E (GPa)194-186-179-172-165-
The yield point, Rp0,2 (MPa)>172>157>147>137>127>120>115>112>110>108
Linear expansion coefficient, α (* 10-6 K-1)16.0-16.5-17.0-17.5-18.0-

 


Heat and plastic treatment of 1.4438, AISI 317L

  • forging and rolling at temperatures 1150 - 800℃
  • Supersaturation at 1020 - 1100 ℃

 


In the 1.4438, AISI 317L grade we deliver:

 


Other grades designations:

X 2 CrNiMo18-15-4, TP317L, 317 L, 1.4438, 1.4476, 317S12, 317 S 12, X3CrNiMo18-16-5, SUS317L, T 7MoNiCr180, UNS S31703, 317-L, Z3CND19-15-04, Z 3 CND 19-15-04.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.