Acid-resistant steel 1.4466, X1CrNiMoN25-22-2, 1.4465, X1CrNiMoN25-25-2, AISI 310MoLN, UNS S31050 according to EN 10088-1.

 

StandardSteel Grade
Chemical Composition %
C:Mn:Si:P:S:Cr:Mo:Ni:N:
EN1.4466 - X1CrNiMoN25-22-2
<0.02<2.0<0.7<0.025<0.01024.0 - 26.02.0 - 2.521.0 - 23.00.10 - 0.16
ASTMUNS S31050 - AISI 310MoLN - 25.22.2
<0.025<2.0<0.5<0.020<0.03024.0 - 26.01.6 - 3.020.5 - 23.50.09 - 0.16
NFZ2CND25-22Az
<0.02<2.0<0.75<0.025<0.01024.0 - 26.02.0 - 2.521.0 - 23.00.10 - 0.16
BS725LN
<0.02<2.0<0.7<0.025<0.01024.0 - 26.02.0 - 2.521.0 - 23.00.10 - 0.16
SEW 4001.4465 - X 1 CrNiMoN 25-25-2 - X1CrNiMoN25-25-2
<0.02<2.0<0.7<0.020<0.01524.0 - 26.02.0 - 2.522.0 - 25.00.08 - 0.16
GOST02Ch25N22AM2 - 02Х25Н22АМ2
<0.021.5 - 2.0<0.4<0.020<0.01524.0 - 26.02.0 - 2.521.0 - 23.00.10 - 0.14

 

1.4466, X1CrNiMoN25-22-2, AISI 310MoLN - specification and application

High-nickel austenitic stainless steel for parts and components of chemical apparatus used mainly in the production of urea. The grade is suitable for working at elevated temperatures. 1.4466 steel is used in the paper, nitrogen, pharmaceutical, petrochemical and cellulose industries.


Mechanical properties of 1.4466, X1CrNiMoN25-22-2, AISI 310MoLN

  • Tensile strength, Rm: 540 - 570 MPa
  • The yield point, Rp0,2: >250 MPa
  • Elongation, A:> 40%
  • Impact resistance, KV: > 60J
  • Modulus of elasticity, E: 190 GPa
  • Thermal capacity, cp: 500 J * kg-1 * K-1
  • Thermal conductivity, λ: 15 W * m-1 * K-1
  • Linear expansion coefficient, α: 15.7 * 10-6 K-1
  • Specific resistance, Ω: 0.8 mkOhm * m

 


Properties at elevated temperatures of 1.4466, X1CrNiMoN25-22-2, AISI 310MoLN:

Temperature (℃)100150200250300350400500
Linear expansion coefficient, α (* 10-6 K-1)15.7---17.0---
Modulus of elasticity, E (GPa)190-182-174-166158
The yield point, Rp0,2 (MPa)>195>170>160>150>140>135--

 


Heat and plastic treatment processes for 1.4466, X1CrNiMoN25-22-2, AISI 310MoLN steel:

  • Supersaturation at 1070 - 1150 ℃
  • Rolling and forging at a temperature of 1150 - 850 ℃

 


In the above-mentioned grades we deliver:

 


Other grades designations:

1.4466, X1CrNiMoN25-22-2, X 1 CrNiMoN 25-22-2, UNS S31050, AISI 310MoLN, 310 MoLN, TP310MoLN, UREA 25.22.2, UNS S35115, 25Cr-22Ni-2Mo-N, 2RE69, 2RM69 WB, 25.22.2.LMn, 725LN, DMV 25.22.2, X2CrNiMoN25-22-2, X 1 CrNiMoN 25-25-2, X1CrNiMoN25-25-2, 1.4465, Z2CND25-22Az, Z1CND25-22Az, 022Cr25Ni22Mo2N, 02Ch25N22AM2, 02Х25Н22АМ2


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.