Unalloyed carbon steel C55S, 1.1204, CS50, Ck55 for thermal improvement according to PN-EN 10132-4.

 

Standards Steel Grades
Chemical Composition %
C: Mn: Si: P: S: Cr: Mo: Ni: Al: Cu:
EN / DIN C55S - 1.1204 - C 55 S - Ck55 - Ck 55 - CS50 - CS 50
0.52 - 0.60 0.60 - 0.90 0.15 - 0.35 <0.025 <0.025 <0.40 <0.10 <0.40 - -
EN 132 2CS55 - 2 CS 55 - 1.1203
0.52 - 0.60 0.60 - 0.90 0.15 - 0.40 <0.035 <0.035 - - - - -
AFNOR C50RR - XC 50 - XC50
0.47 - 0.52 0.50 - 0.80 0.15 - 0.35 <0.025 <0.020 <0.30 <0.10 <0.40 <0.03 -
BS CS50 - CS 50
0.45 - 0.55 0.50 - 0.90 0.05 - 0.35 <0.045 <0.045 - - - - -
IS 55C6
0.50 - 0.60 0.50 - 0.65 0.15 - 0.35 <0.05 <0.05 - - - - -
EN C55E - 1.1203
0.52 - 0.60 0.60 - 0.90 <0.40 <0.03 <0.035 <0.40 <0.10 <0.40 - -
PN 55 - gat. 55
0.52 - 0.60 0.60 - 0.90 0.10 - 0.40 <0.04 <0.04 <0.30 <0.10 <0.30 - <0.30

 

C55S, 1.1204 - specification and application

Spring steel with low hardening capacity designed for lightweight springs and springs, washers and spring elements, small tool blades, small dimensions equipment with carbon range of approx. 0.55% for heat improvement, patenting or cold deformation.

Supplied in the form of cold-rolled tapes and wires for oil hardening. After heat treatment, the steel exhibits a tempered martensite structure and is prone to decarburizing and oxidation during heat treatment.


Mechanical properties of C55S

echanical properties according to EN 10132-4
Soft state after smoothing rolling +A +LC
Tensile strength Rm < 600 MPa
Yield point Re < 480 MPa
Elongation A > 17%
Hardness < 185 HV < 90 HB
Condition after cold plastic deformation +CR
Tensile strength Rm < 1070 MPa
Hardness < 300 HV
Condition after hardening and tempering in oil
Tensile strength Rm 1100 - 1700 MPa
Hardness HV HRC 340 - 520 HV 34.0 - 50.50 HRC
Density ρ 7.82 kg/dm³

 


In the C55S grade the company provides:

 


Other grades of spring steel:

C55S, 1.1204, C 55 S, Ck55, Ck 55, CS50, CS 50, 2CS55, 2 CS 55, 1.1203, C50RR, XC 50, XC50, CS50, CS 50, 55C6, C55E, 1.1203, 55, gat. 55


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.