C125S, 1.1224, XC125 - Spring low-alloy carbon steel for heat treatment - hardening in oil, according to EN 10132-4 i EN 10270-1.

Standard Steel grade
Chemical Composition %
C: Mn: Si: P: S: Cr: Mo: Ni: Al: Cu:
EN/DIN C125S - 1.1224 - C 125 S
1.20 - 1.30 0.30 - 0.60 0.15 - 0.35 <0.025 <0.025 <0.40 <0.1 <0.40 - -
AFNOR C125RR - C 125 RR - XC125 - XC 125
1.20 - 1.30 0.30 - 0.60 0.15 - 0.30 <0.025 <0.020 <0.30 <0.1 <0.40 <0.03 -
IS 115C5
1.10 - 1.20 0.40 - 0.60 0.10 - 0.35 <0.04 <0.04 <0.20 - - <0.25 -
EN/DIN 125Cr1 - 125 Cr 1 - 125Cr2 - 125 Cr 2 - 1.2002 - 2002
1.20 - 1.30 0.25 - 0.40 0.15 - 0.35 <0.025 <0.025 0.40 - 0.60 <0.1 <0.40 - -
AFNOR C120E3UCr4 - Y2 120 C
1.10 - 1.29 0.10 - 0.40 0.10 - 0.30 <0.025 <0.025 0.20 - 0.50 - - - -
AFNOR XC130 - XC 130
1.20 - 1.35 0.30 - 0.45 0.20 - 0.35 <0.030 <0.025 0.20 - 0.50 - - - -
JIS SKS 81 - SKS81 - SKS 81 M - SKS81M - TE-2
1.10 - 1.30 <0.50 <0.35 <0.030 <0.030 0.20 - 0.50 - <0.25   <0.25

 


Steel C125S, 1.1224 - implementation and specification

Non-alloy carbon spring steel is used for leaf springs and springs with small cross-sections. It is characterized by low hardenability and high carbon range in relation to C90S, C75S, C85S, and C67S steel. Designed for spring elements requiring high elasticity and hardness.

It does not show corrosion resistance, and during heat treatment it is exposed to decarburization and oxidation, which means that the material should be protected against treatment using a protective atmosphere. Poorly carried out treatment is associated with reduced fatigue strength.

Products made of C125S steel and its equivalents are produced in the form of flat semi-finished products - cold rolled strips, small-format thin sheets. Tempering of C125S steel is carried out in oil, and after tempering the product shows the structure of tempered martensite.

Products made of C125S steel are characterized by high tensile strength and yield strength. Thermal improvement consists in austenitising the product at a temperature of 780 - 860 and tempering at a temperature of 350 - 500 ℃.


Mechanical properties of steel C125S (1.1224)

Mechanical properties
The softened condition after smoothing rolling C125S +A+LC
Tensile strength Rm < 740 MPa
The yield point Re < 600 MPa
Elongation A > 11%
Hardness HV HRB < 230 HV < 97 HRB
Cold-rolled condition C125S +CR
Tensile strength Rm < 1200 MPa
Hardness HV < 325 HV
Heat-treated condition C125S +QT
Tensile strength Rm 1200 - 2100 MPa
Hardness HV HRC 370 - 630 HV 38.5 - 57.0 HRC

 


In the grade of 1.1224 C125S, the company offers:

 


The list of equivalents and other designations of C125S, (1.1224) steel:

C 125 S, C125RR, C 125 RR, XC125, XC 125, 115C5, 125Cr1, 125 Cr 1, 125Cr2, 125 Cr 2, 1.2002, 2002, C120E3UCr4, Y2 120 C, XC130, XC 130, SKS 81, SKS81, SKS 81 M, SKS81M, TE-2


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.