Structural alloy steel 30NiCrMo12, 30NCD12, 32NiCrMo12-5, 32NiCrMo10-4, 1.6655, 1.6743 for heat treatment for particularly stressed parts for aircraft industry according to UNI 6924.

 

StandardsSteel Grades
Chemical Composition %
C:Mn:Si:P:S:Cr:Ni:Mo:V:
UNI 692430NiCrMo12 - 30 NiCrMo 12
0.28 - 0.340.5 - 0.8<0.4<0.025<0.0200.6 - 0.92.7 - 3.20.40 - 0.60-
AFNOR30NCD12 - 30 NCD 12
0.25 - 0.350.15 - 0.550.1 - 0.4<0.030<0.0250.7 - 1.12.8 - 3.20.25 - 0.45-
DIN32NiCrMo12-5 - 32 NiCrMo 12-5 - 1.6655
0.29 - 0.360.25 - 0.500.15 - 0.40<0.025<0.0251.2 - 1.52.8 - 3.00.30 - 0.40-
DIN32NiCrMo10-4 - 32 NiCrMo 10-4 - 1.6743
0.28 - 0.360.30 - 0.600.15 - 0.35<0.035<0.0350.9 - 1.22.4 - 2.70.35 - 0.55-
BS826M31 - 826 M 31
0.27 - 0.350.45 - 0.700.10 - 0.40<0.035<0.0400.5 - 0.82.3 - 2.80.45 - 0.65-
ASTMA723 Grade 2 - UNS K34035
<0.40<0.90<0.35<0.015<0.0150.8 - 2.02.3 - 3.30.30 - 0.50<0.2

 

Steel 30NiCrMo12 - application

30NiCrMo12 steel is a typical alloy construction grade for heat treatment - hardening and tempering, which is characterized by very high mechanical properties, hardness, load resistance and variable pressure.

Steel is used i.e. in aviation as well as for components and particularly responsible components of machinery, equipment, vehicles such as axles, couplings, shafts, levers or connecting rods.


Mechanical properties of 30NiCrMo12 steel

  • Tensile strength, Rm: 880 - 1180 MPa
  • Yield point, Re: > 685 MPa
  • Elongation, A: 14%
  • Notch toughness, KCU: 35 - 40 J
  • Hardness in softened state < 260 HB

 


Heat treatment - processes and temperatures

  • Softening annealing with isothermal transformation at 800℃, with cooling at 620℃ for 24 hours
  • Normalizing annealing at 840 - 870℃
  • Relief annealing at 640 - 670℃
  • Hardening with cooling in oil at the temperature of 830 - 850 ℃
  • Tempering at 550 - 650℃

 


In the above mentioned grades the company provides:


Other signs and equivalents:

30NCD12, 30 NCD 12, TALABOT 30 NCD 12, 32NiCrMo12-5, 1.6743, 32 NiCrMo 12-5, 1.6655, A 723 Grade 2, ASTM A723, K34035, S-23093A, 30NCD11, 30 NCD 11, 30NCD15, 30 NCD 15, 826M31, 826 M 31, S.153, F-127, 32NiCrMo14-5, 32 NiCrMo 14-5, 1.6746, 30NiCrMo12, 30 NiCrMo 12


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.