18H2N2, 18CrNi8, 1.5920 - case-hardening alloy steel for carburizing according to PN-H-84030, DIN 17210.

 

Standard Steel Grade
Chemical Composition %
C: Mn: Si: P: S: Cr: Ni: Al: Ti: Cu:
PN 18H2N2
0.15 - 0.22 0.4 - 0.7 0.17 - 0.37 <0.035 <0.035 1.8 - 2.1 1.8 - 2.1 - - <0.3
DIN 18CrNi8 - 1.5920
0.15 - 0.20 0.4 - 0.6 0.15 - 0.40 <0.035 <0.035 1.8 - 2.1 1.8 - 2.1 <0.2 - -
STAS 18CrNi20
0.17 - 0.22 0.8 - 1.0 0.15 - 0.40 <0.035 <0.035 1.8 - 2.1 1.8 - 2.1 - <0.02 <0.3
UNE F-150.E - A-150.E
0.13 - 0.19 0.35 - 0.65 0.13 - 0.38 <0.035 <0.035 1.85 - 2.15 1.85 - 2.15 - - -
NF 18CN8
0.25 - 0.20 0.4 - 0.6 0.15 - 0.40 <0.035 <0.035 1.8 - 2.1 1.8 - 2.1 - - -

 


18H2N2, 18CrNi8, 1.5920 - specifications and applications

Structural steel for carburizing with high content of chromium and nickel, designed for particularly stressed parts of machines with large cross-sections, which require high strength, resistance to variable loads, fatigue, impact resistance and ductility of the core. Used in the production of large gears, disc wheels, pivots, shafts in the machine industry, grade 18H2N2 achieves surface hardness in the range of 59 - 65 HRC after carburizing.

 


Mechanical properties of 18CrNi8 / 18H2N2

  • Tensile strength, Rm: 1230 - 1470 MPa
  • Yield strength, Re: >830 MPa
  • Elongation, A: >7%
  • Necking, Z: >30%
  • Hardness in annealed condition: <235 HB

 


Heat treatment processes of 18CrNi8 / 18H2N2 steel

  • Softening annealing at 650 - 700℃
  • Normalising annealing at 870 - 900℃
  • Carburizing at 880 - 950℃
  • Carbonitriding at 860 - 930℃
  • Hardening I in water or oil after carburizing at 840 - 870℃
  • Annealing after carburizing at 630 - 650℃
  • Hardening II in water or oil after carburizing at 800 - 830℃
  • Tempering at 170 - 200℃

 


In the above mentioned grades we offer:

 


Other designations and equivalents:

18CrNi8, 18 CrNi 8, 1.5920, 18 CN 8, 18CN8, 18CrNi20, 18 CrNi 20, F-150.E, A-150.E


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.