X11CrMo9-1, X12CrMo9-1, 1.7386 - high-alloy boiler steel for operation at elevated temperatures according to EN 10216-2, A213/A335.

Standard Steel Grade
Chemical composition
C: Mn: Si: P: S: Cr: Ni: Mo: Al: Cu:
EN X11CrMo9-1 - 1.7386
0.08 - 0.15 0.3 - 0.6 0.25 - 1.00 <0.025 <0.010 8.0 - 10.0 - 0.9 - 1.1 <0.4 <0.3
DIN X12CrMo9-1 - 1.7386
0.07 - 0.15 0.3 - 0.6 0.25 - 1.00 <0.025 <0.020 8.0 - 10.0 - 0.9 - 1.1 - -
GOST 13Ch9M - 13Х9М
0.09 - 0.15 <0.5 <0.5 <0.035 <0.025 7.5 - 9.5 <0.5 0.9 - 1.1 - <0.25
ASTM UNS K90941 - A213 T9 - A335 P9 - A387 Grade 9
<0.15 0.3 - 0.6 0.25 - 1.00 <0.030 <0.030 8.0 - 10.0 - 0.9 - 1.1 - -
JIS STBA26 - STFA26 - STPA26
<0.15 0.3 - 0.6 0.25 - 1.00 <0.030 <0.030 8.0 - 10.0 - 0.9 - 1.1 - -

X11CrMo9, 1.7386 - specification and application

High alloy boiler steel for operation at elevated temperatures supplied in the form of pipes, flanges, bars and forgings with a chromium content of 9% and 1% of Molybdenum. The material shows a martensitic structure after tempering and ferritic structure in the annealed state, it is characterized by high resistance to creep/oxidation and cracks and low thermal expansion. Steel designed for operation at temperatures of 550-650C for power and petrochemical industry for pipelines, secondary and outlet steam superheaters, steam and outlet collectors, turbine parts, flanges, connectors, and heat exchangers. Grade close to 1.4903 / F91 / P91 without added Niobium and Vanadium.


Mechanical properties of X11CrMo9, 1.7386 pipes according to EN 10216-2

  • Delivery condition +I:
    • Tensile strength, Rm 460 - 640 MPa
    • Yield strength, Rp0,2: >210 MPa
    • Longitudinal tests - Elongation, A: >20%
    • Longitudinal tests - Impact strength, KV: >40J
    • Lateral tests - Elongation, A: >18%
    • Lateral tests - Impact strength, KV: >27J
  • Delivery condition +NT:
    • Tensile strength, Rm 590 - 740 MPa
    • Yield strength, Rp0,2: >390 MPa
    • Longitudinal tests - Elongation, A: >18%
    • Longitudinal tests - Impact strength, KV: >40J
    • Lateral tests - Elongation, A: >16%
    • Lateral tests - Impact strength, KV: >27J

Mechanical properties of UNS K90941, grade 9

  • ASTM A335 Grade P9 / A213 Grade T9
    • Tensile strength, Rm >415 MPa
    • Yield strength, Rp0,2: >205 MPa
    • Longitudinal tests - Elongation, A: >30%
    • Lateral tests - Elongation, A: >20%
    • Hardness HV: <190
    • Hardness HRB: <89
    • Hardness HBW: <179
  • ASTM A336 Grade F9:
    • Tensile strength, Rm  585 - 760 MPa
    • Yield strength, Rp0,2: >380 MPa
    • Elongation, A: >20%
    • Necking, Z: >40%
  • ASTM A182 Grade F9
    • Tensile strength, Rm  >585 MPa
    • Yield strength, Rp0,2: >380 MPa
    • Elongation, A: >20%
    • Necking, Z: >40%
    • Hardness: 179 - 217HB

Mechanical properties of X11CrMo9-1 at elevated temperatures

Yield strength, Rp0.2 (MPa)
Temp. in C 100 150 200 250 300 350 400 450 500 550
X11CrMo9+I >187 >186 >178 >177 >175 >171 >164 >153 >142 >120
X11CrMo9+NT >363 >348 >334 >330 >326 >322 >316 >311 >290 >235

Heat treatment - processes and temperatures:

  • Softening annealing at the temperature of 950-980C
  • Nitriding at the temperature of 890-950C
  • Tempering at temperature 720-800C

In the above mentioned grades the company offers:


Other substitutes and grade equivalents:

X12CrMo9-1, 1.7386, X11CrMo9-1+I, X11CrMo9-1+NT, X11CrMo9-1TA, X11CrMo9-1TN, X11CrMo9-1TN+TT, X11CrMo9, BS629-470, BS629-590, CromElso 9, 13Ch9M, 13Х9М, UNS K90941, A213 grade T9, A335 grade P9, EN 10253-2, A387 Grade 9, STBA26, STFA26, STPA26, HT7R, A182 F9, A200 T9, A387 Grade 9, A369 Grade FP9, A182 grade F9, 9Cr-1Mo.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.