High-alloyed chrome-molybdenum boiler steel with the addition of Niobium, Vanadium and Boron X19CrMoNbVN11-1, 1.4913 according to EN 10088-1, EN 10302 and EN 10269.

 

Standard Steel Grade
Chemical Composition %
C: Mn: Si: P: S: Cr: Ni: Mo: V: Nb: Al: W: B: N: Cu: Ti:
EN X19CrMoNbVN11-1 - 1.4913 - X 19 CrMoNbVN 11-1
0.17 - 0.23 0.4 - 0.9 <0.5 <0.025 <0.015 10.0 - 11.5 0.2 - 0.6 0.5 - 0.8 0.1 - 0.3 0.25 - 0.55 <0.02 <0.7 0.005 - 0.015 0.05 - 0.10 - -
BN 17H11MFNb
0.15 - 0.21 0.6 - 1.0 <0.6 <0.030 <0.035 10.0 - 11.5 0.5 - 1.0 0.8 - 1.1 0.20 - 0.45 0.20 - 0.45 - - - - - -
NF Z20CDNbV11 - Z 20 CDNbV 11 - 56T5 - 56 T 5
0.18 - 0.25 0.3 - 0.8 0.1 - 0.5 <0.025 <0.015 10.0 - 12.0 <1.0 0.5 - 1.0 0.1 - 0.3 0.25 - 0.55 - - - 0.05 - 0.10 - -
NF Z21CDNbV11 - Z 21 CDNbV 11
0.16 - 0.25 0.3 - 0.8 0.1 - 0.5 <0.030 <0.015 10.0 - 12.0 <1.0 0.5 - 1.0 0.1 - 0.3 0.25 - 0.55 - - - 0.05 - 0.10 - -
ISO X18CrMnMoNbVN12 - MM12G - 1.4916
0.15 - 0.20 0.5 - 1.0 <0.5 <0.040 <0.030 10.0 - 13.0 <0.6 0.3 - 0.9 0.1 - 0.4 0.2 - 0.6 - - - 0.05 - 0.10 - -
GOST 18Ch11MNFB - 18Х11МНФБ - 2Х11МФБН - ЕП291
0.15 - 0.21 0.6 - 1.0 <0.6 <0.030 <0.025 10.0 - 11.5 0.5 - 1.0 0.8 - 1.1 0.2 - 0.4 0.20 - 0.45 - <0.2 - - <0.3 <0.2

 


X19CrMoNbVN11-1, 1.4913 - specification and application

High-alloy boiler heat-resistant steel designed for thermal improvement and nitriding. When working at elevated temperatures resistant to 600 ℃, characterized by good resistance and creep limit. It is used for the production of bolts, nuts, fasteners, discs and turbine rotors in the energy, maritime and aerospace industries, as well as injection elements. Steel is difficult to weld.


Mechanical properties of X19CrMoNbVN11-1, 1.4913 +QT

Properties according to EN 10088-1, EN 10269, EN 10302 in condition + QT for sections <160mm

  • Tensile strength, Rm: 900 - 1050 MPa
  • The yield point, Re: > 750 MPa
  • Elongation, A:> 12%
  • Contraction, Z: >40%
  • Impact resistance, KV20℃: >20J
  • Modulus of elasticity, E: 216 GPa
  • Thermal capacity, cp20℃: 460 J * kg-1 * K-1
  • Thermal conductivity, λ: 24,0 W * m-1 * K-1
  • Linear expansion coefficient, α: 10,5 * 10-6 K-1

 

Mechanical properties at elevated temperatures

Properties Temperature (℃)
50 100 150 200 250 300 350 400 450 500 550 600
The yield point Rp0.2 (MPa) >726 >701 >676 >651 >643 >627 >610 >577 >544 >495 >412 >305

 


In the above mentioned grade, the company provides:

 

Other indications:

18Cr11NiMoNbVN, 18Cr12MoVNbN, 2Cr11NiMoNbVN, 1.4916, 17H11MFNb, Z20CDNbV11, Z 20 CDNbV 11, Z21CDNbV11, Z 21 CDNbV 11, MM12G, 4916-600-77-J, X18CrMnMoNbVN12, X 18 CrMnMoNbVN 12, SUH600, F SUH 600, X19CrMoNbVN11-1, X 19 CrMoNbVN11-1, 1.4913, 56 T 5, 56T5, 1.4916, 18Ch11MNFB, 18Х11МНФБ, 2Х11МФБН, ЕП291.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.