Low-alloy bioler carbon steel bars P250GH, C22.8, 1.0460 for operation at elevated temperatures for pressure equipment according to EN 10273, DIN 17243.

 

Standard Steel Grade
Chemical Composition %
C: Mn: Si: P: S: Cr: Ni: Mo: V: Nb: Ti: Alc: Cu: N:
EN P250GH - P 250 GH - 1.0460
0.18 - 0.23 0.3 - 0.9 <0.4 <0.025 <0.015 <0.3 <0.3 <0.08 <0.02 <0.02 <0.03 >0.02 <0.3 <0.012
DIN C22.8 - C 22.8 - C22G2 - C 22 G 2
0.18 - 0.23 0.3 - 0.9 <0.4 <0.025 <0.015 <0.3 <0.3 <0.08 <0.02 <0.02 <0.03 >0.02 <0.3 <0.012
EN P265GH - P 265 GH - 1.0425
<0.2 0.5 - 1.4 <0.4 <0.030 <0.025 <0.3 <0.3 <0.08 <0.02 <0.02 <0.03 >0.02 <0.3 <0.012
PN St36K
0.08 - 0.16 >0.4 0.15 - 0.35 <0.045 <0.045 <0.3 <0.3 - - - - - <0.3 -
PN St41K
0.12 - 0.20 >0.45 0.15 - 0.35 <0.045 <0.045 <0.3 <0.3 - - - - - <0.3 -
PN St44K
0.14 - 0.22 >0.55 0.15 - 0.35 <0.045 <0.045 <0.3 <0.3 - - - - - <0.3 -

 


P250GH, C22.8, 1.0460 - application

Boiler steel designed to operate at elevated temperature for many parts and subassemblies of pressure equipment operating up to 450 ℃, such as parts of pressure vessels, bolts, nuts, flanges, pipe joints and other power installations. P250GH is a grade in which mainly hot-rolled rods are supplied in the normalized state.

 


Mechanical properties of P250GH, C22.8, 1.0460 +N

  • Dimensions < 50mm
    • Tensile strength, Rm: 410 - 540 MPa
    • The yield point, Rp,02 > 250 MPa
    • Elongation, A > 25%
  • Dimensions 50 - 100mm
    • Tensile strength, Rm: 410 - 540 MPa
    • The yield point, Rp0,2 > 240 MPa
    • Elongation, A > 25%
  • Dimensions 100 - 150mm
    • Tensile strength, Rm: 410 - 540 MPa
    • The yield point, Rp0,2 > 230 MPa
    • Elongation, A > 25%
  • Impact energy, KV20℃ > 47 J

 


Mechanical properties at individual operating temperatures:

The yield point Rp0,2 (MPa) Temperature
50℃ 100℃ 150℃ 200℃ 250℃ 300℃ 350℃ 400℃ 450℃
Dimensions <50mm >242 >237 >216 >190 >170 >150 >130 >110 >90
Dimensions 50 - 100mm >234 >230 >210 >185 >165 >145 >125 >100 >80
Dimensions 100 - 150mm >224 >220 >200 >175 >155 >135 >115 >90 >70

 


Heat treatment of P250GH steel

  • Normalizing at 890 - 950 ℃
  • Relief annealing at a temperature of 520 - 580℃

In the above mentioned grades the company provides:

 


Other grades designations:

St36K, St41K, St44K, P250GH, P235GH, P265GH, C22.8, C 22.8, C 22 G 2, C22G2, 1.0460, 1.0425, P265, SPV355.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.