High-speed tungsten steel with addition of vanadium 1.3355, HS18-0-1, AISI T1 according to ISO 4957.

 

Standard Steel Grade
Chemical Composition %
C: Mn: Si: P: S: Cr: Ni: Mo: V: W: Co:
PN SW18
0.75 - 0.85 <0.4 <0.5 <0.03 <0.03 3.5 - 4.5 <0.4 - 1.0 - 1.4 17.0 - 19.0 <0.3
ISO HS18-0-1 - 1.3355
0.73 - 0.83 <0.4 <0.45 <0.03 <0.03 3.8 - 4.5 - - 1.0 - 1.2 17.2 - 18.7 -
ASTM AISI T1 - UNS T12001 - AMS 5626
0.65 - 0.80 0.1 - 0.4 0.2 - 0.4 <0.03 <0.03 3.75 - 4.50 - - 0.9 - 1.3 17.25 - 18.75 -
NF Z80WCV18-04-01
0.75 - 0.83 <0.4 <0.5 <0.03 <0.03 3.5 - 4.5 - 1.00 - 1.30 - 17.2 - 18.7 -
GOST R18 - Р18
0.73 - 0.83 <0.5 <0.5 <0.03 <0.03 3.8 - 4.4 <0.4 <1.0 1.0 - 1.4 17.0 - 18.5 <0.5

 

HS18-0-1, 1.3355, AISI T1 - specification and application

High-speed steel with good ductility, machinability and hardness up to 63 HRC used for roughing and finishing tools with medium strength parameters.

SW18 can be used for the production of turning tools, chisel cutters, turning and planing, milling cutters, drill bits, threading tools, saw segments, planer knives, small circular saws, reamers, taps working on automatic machines, and screw cutters.


Mechanical properties of HS18-0-1, 1.3355, AISI T1

  • Hardness in +A delivery condition: <269 HB
  • Hardness in +A+C delivery condition: <319 HB
  • Hardness in +A+CR delivery condition: <339 HB
  • Hardness after hardening and tempering:
    • at 300 ℃ = 63 HRC
    • at 350 ℃ = 60,5 HRC
    • at 400 ℃ = 60,5 HRC
    • at 450 ℃ = 63 HRC
    • at 500 ℃ = 65 HRC
    • at 550 ℃ = 65 HRC
    • at 600 ℃ = 60,5 HRC
    • at 650 ℃ = 57,5 HRC
    • at 700 ℃ = 48 HRC

 


Heat and plastic treatment of HS18-0-1, 1.3355, AISI T1 - processes and temperatures

  • Softening annealing at a temperature of 800 - 900 ℃
  • Relief annealing at a temperature of 600 - 700℃
  • Heating no. I in a temp. of about 550℃
  • Heating no. II in a temp. of about 850℃
  • Austenitizing at 1230 - 1270 ℃ (hardening in salt bath and oil)
  • Tempering usually in the range of 550 - 570 ℃
  • Tempering usually in the range of 550 - 570 ℃
  • Nitriding in the temperature range of 510 - 530 ℃

 


In the above mentioned grades the company provides:

 


Other indications of grades and substitutes:

HS18-0-1, HS 18-0-1, AISI T1, AISI T-1, UNS T12001, AMS 5626, CSN 19824, SS 2750, SS2750, SKH2, SKH 2, BT1, RP3, R3, ST SEW 44850, W18Cr4V, X75WCrV18-4-1, 1.3558, Z80WCV18-04-01, R18, Р18.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.