Stainless super duplex steel 1.4507 / S32550 with two-phase structure for chemical industry according to EN 10088-1.

Standard Steel Grade
Chemical Composition %
C: Mn: Si: P: S: Cr: Mo: Ni: Cu: N:
EN 1.4507 - X2CrNiMoCuN25-6-3
<0.03 <2.0 <0.7 <0.035 <0.015 24.0 - 26.0 3.0 - 4.0 6.0 - 8.0 1.0 - 2.5 0.20 - 0.30
ASTM UNS S32550 - A182 grade F61 - Alloy 255
<0.04 <1.5 <1.0 <0.040 <0.030 24.0 - 27.0 2.9 - 3.9 4.5 - 6.5 1.5 - 2.5 0.10 - 0.25
ASTM UNS S32520 - A182 grade F59
<0.03 <1.5 <0.8 <0.035 <0.020 24.0 - 26.0 3.0 - 5.0 5.5 - 8.0 0.5 - 3.0 0.20 - 0.35
JIS SUS329J4L - SUS 329J4L
<0.03 <1.5 <1.0 <0.040 <0.030 24.0 - 26.0 2.5 - 3.5 5.5 - 7.5 - 0.08 - 0.30

 

Specification and application

Special grade from the group of super-strong acid-resistant stainless steels similar to 1.4410 / X2CrNiMoN25-7-4 / UNS S32750. The steel exhibits high strength properties with relatively high resistance to various types of corrosion, including intergranular corrosion. 1.4507 and UNS S32550 materials are used in the paper, chemical, nitrogen, and aviation industries as well as in power engineering for screws, shafts, sleeves, fittings, installations and pipelines, pump parts, tanks for chemicals, heat exchangers, radiator parts and aircraft constructions .


Mechanical properties

  • Tensile strength, Rm: 700 - 900 MPa
  • The yield point, Rp0,2: >500 MPa
  • Elongation, A:> 25%
  • Modulus of elasticity, E: 200 GPa
  • Hardness, HB: <270
  • Thermal capacity, cp: 500 J * kg-1 * K-1
  • Thermal conductivity, λ: 15 W * m-1 * K-1
  • Linear expansion coefficient, α: 13.0 * 10-6 K-1
  • Specific resistance, Ω: 0.8 mkOhm * m

Mechanical properties at elevated temperature

Temperature (℃) 100 150 200 250 300
Linear expansion coefficient, α (* 10-6 K-1) 13.0 - 13.5 - 14.0
Modulus of elasticity, E (GPa) 194 - 186 - 180
The yield point, Rp0,2 (MPa) >450 >420 >400 >380 -

Heat and plastic treatment of UNS S32550 / 1.4507

  • Supersaturation at 1020 - 1100 ℃
  • Rolling and forging at a temperature of 1200 - 900 ℃

In the above-mentioned grades we deliver:


Other grades designations:

1.4507, X2CrNiMoCuN25-6-3, F59, 03Cr25Ni6Mo3Cu2N, 52N+, X3CrNiMoCuN26-6-3-2, UR52N, SUS329J4L, SUS 329J4L, UNS S32520, Grade 255, Super Duplex 255, Alloy 255, UNS S39553.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.