Heat-resistant boiler steel H6S2, X10CrAl7, X10CrAlSi7, 1.4713 according to EN 10095, EN 10088-1, SEW 470, PN-71/H-86022.

 

Standard Steel Grade
Chemical Composition %
C: Mn: Si: P: S: Cr: Ni: Al: Cu:
EN/DIN 1.4713 - X10CrAl7 - X10CrAlSi7
<0.12 <1.0 0.5 - 1.0 <0.04 <0.015 6.0 - 8.0 - 0.5 - 1.0 -
DIN 1.4712 - X10CrSi6
<0.12 <1.0 2.0 - 2.5 <0.045 <0.030 5.5 - 6.5 - - -
PN H6S2
<0.15 <0.7 1.5 - 2.0 <0.040 <0.030 5.0 - 6.5 <0.6 - <0.3
GOST 15Х6СЮ
<0.15 <0.5 1.2 - 1.8 <0.03 <0.025 5.5 - 7.0 - 0.7 - 1.1 -

 

X10CrAl7, X10CrAlSi7, 1.4713 - specifications and application

H6S2 is a ferritic heat-resistant steel showing resistance to sulfur compounds, reducing and carburizing gases, which can operate in temperatures up to 800 in a non-aggressive environment.

It is used in the production of load-bearing elements, parts of steam boilers, construction of soot blowers, supports for heaters, hubcaps, sliding rails, chains and sieves, parts in the automotive, energy and metallurgical industries.

The grade during welding and after the joining process requires heating. The steel is resistant to light loads during continuous operation.


Mechanical and physical properties of X10CrAl7, 1.4713 steel

  • Tensile strength, Rm: 420 - 620 MPa
  • The yield point, Rp0,2: >220 MPa
  • Elongation, A:> 15%
  • Hardness, HB: <192
  • Specific resistance, Ω: 0.70 mkOhm * m
  • Linear expansion coefficient, α: 11.5 - 13.0 * 10-6 K-1
  • Thermal conductivity, λ: 23.0 W * m-1 * K-1
  • Thermal capacity, cp: 450 J * kg-1 * K-1

 


Mechanical properties at elevated temperatures of X10CrAl7, 1.4713

Temperature (℃) 500 600 700 800 900
Creep strength, Rz/1000 (MPa) 160 55 17 7.5 3.6
Creep strength, Rz/10000 (MPa) 100 35 9.5 4.3 1.9
Creep strength, Rz/100000 (MPa) 55 20 5 2.3 1.0
Creep limit, R1/1000 (MPa) 80 27.5 8.5 3.7 1.8
Creep limit, R1/10000 (MPa) 50 17.5 4.7 2.1 1.0

 


Heat and plastic treatment of H6S2, X10CrAl7, 1.4713

  • Annealing at 780 - 840℃ with cooling in water or air

 


In the H6S2 grade and its replacement, we offer:

 


Other grades designations:

4713, Sicromal, X 10 CrAl 7, X 10 CrAlSi 7, X10CrSi6, X 10 CrSi 6, 1.4712, CSN 17113, 15Ch6SJU, 15Х6СЮ, 10AlCr70.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.