Boiler steel for power engineering 10CrMo9-10, 1.7380, ASTM F22/P22 designed for use at elevated temperatures on pressure equipment according to EN 10273 and EN 10216-2.

 

Standards Steel Grades
Chemical Composition %
C: Mn: Si: P: S: Cr: Mo: V: Ni: Al: Cu: N:
PN 10H2M
0.08 - 0.15 0.4 - 0.6 0.15 - 0.50 <0.030 <0.030 2.0 - 2.5 0.9 - 1.1 - <0.3 <0.02 <0.25 -
EN 10CrMo9-10 - 10 CrMo 9-10 - 1.7380
0.08 - 0.14 0.4 - 0.8 <0.50 <0.020 <0.010 2.0 - 2.5 0.9 - 1.1 - - - <0.30 -
EN 11CrMo9-10 - 11 CrMo 9-10 - 1.7383
0.08 - 0.15 0.4 - 0.8 <0.50 <0.025 <0.015 2.0 - 2.5 0.9 - 1.1 - - - - -
EN 12CrMo9-10 - 12 CrMo 9-10 - 1.7375
0.10 - 0.15 0.3 - 0.8 <0.30 <0.015 <0.010 2.0 - 2.5 0.9 - 1.1 - <0.3 0.01 - 0.04 <0.25 <0.012
GOST 10Ch2M - 10Х2М - 10Kh2M - 1Ch2M - 1Kh2M - 1Х2М
0.08 - 0.12 0.4 - 0.7 0.17 - 0.37 <0.020 <0.020 2.0 - 2.5 0.6 - 0.8 - <0.3 <0.02 <0.20 -
ČSN
STN
ČSN 15 313 - ČSN 15313
0.08 - 0.15 0.4 - 0.8 0.15 - 0.40 <0.035 <0.035 2.0 - 2.5 0.9 - 1.1 - - - - -
AFNOR 10CD9-10 - 10 CD 9-10
<0.15 0.3 - 0.6 <0.35 <0.020 <0.015 2.0 - 2.5 0.9 - 1.1 <0.04 - - <0.30 -
AFNOR 12CD9-10 - 12 CD 9-10
<0.16 0.3 - 0.6 0.10 - 0.40 <0.015 <0.012 2.0 - 2.5 0.9 - 1.1 <0.03 <0.3 - - -
UNS 
ASTM
K21590 - 2.25Cr1Mo - A182 F22 - A182 T22
0.05 - 0.15 0.3 - 0.6 <0.50 <0.040 <0.040 1.9 - 2.6 0.87 - 1.13 <0.02 - - - -
UNS K21390
0.05 - 0.15 0.3 - 0.6 <0.50 <0.025 <0.025 2.0 - 2.5 0.9 - 1.1 <0.05 <0.5 - - -

 

Low-alloy steel 10CrMo9-10, 1.7380 - description and specification

Chrome-manganese, perlitic creep resistant structural steel for high temperature applications up to 580 ℃ produced in the form of sheets, forgings, forged bars, hot-rolled tubes, and fittings for the power industry.

It is used, inter alia, for parts of steam boilers, turbine parts, superheat tubes, line pipes and boiler tubes, outlet chambers' parts, coils and superheater chambers, superheated steam pipes, steam coolers, boiler drums, nozzles, caps, screws, stressed parts in the chemical industry, pressure vessels in energy installation.

Compared to other boiler steels, 10CrMo9-10, 1.7380 steel is characterized by M23C6 carbide emissions, and hydrogen degradation resistance in medium pressure equipment and devices up to 500 ℃. In the 10H2M grade the products are generally used in a heat-treated or normalized state.


Mechanical properties in normalized state for individual dimensions

Property Dimensions
do 16mm 16 - 40mm 40 - 60mm 60 - 100mm 100 - 150mm
Normalized state
Tensile strenght Re 480 - 630 MPa 470 - 620 MPa 460 - 610 MPa
Yield point Rp0,2 > 310 MPa  > 300 MPa > 290 MPa > 270 MPa > 250 MPa
Notch toughness KV20℃ > 31 J > 27 J
Elongation A > 18 % > 17 %
Dimensions Heat-treated condition
60 - 100mm 100 - 150mm 150 - 250mm
Tensile strength Re 470 - 620 MPa 460 - 610 MPa 450 - 600 MPa
Yield point Rp0,2 > 280 MPa > 260 MPa > 250 MPa
Notch toughness KV20℃ > 27 J > 27 J > 27 J
Elongation A > 17 % > 17 % > 17 %

 


Thermal treatment 1.7380, 10CrMo9-10

  • Normalizing with cooling in calm air at the temperature of 930 - 960℃
  • Softening annealing with cooling in calm air at the temperature of 730 - 760 ℃
  • Hardening with cooling in oil at the temperature of 920 - 950 ℃
  • Tempering with cooling in calm air at the temperature of 730 - 760 ℃
  • Isothermal treatment with cooling in calm air at 930 - 960 ℃

 


Mechanical properties at specified temperatures

Properties Temperatures
450℃ 480℃ 510℃ 540℃ 570℃ 600℃
Creep limit R1/100000 166 130 90 58 35 22
Creep resistance Rz/100000 221 170 118 78 51 34

 


In 10CrMo9-10, 1.7380 grades we supply:

 


Other signs and equivalents of 10CrMo9-10 boiler steel:

10CrMo9-10, 1.7380, 11CrMo9-10, 1.7383, 12CrMo9-10, 1.7375, 10Ch2M, 10 CrMo 9-10, 11 CrMo 9-10, 12 CrMo 9-10, ČSN 15 313, ČSN 15313, 10Х2М, 10Kh2M, 1Ch2M, 1Kh2M, 1Х2М, 10CD9-10, 10 CD 9-10, 12CD9-10, 12 CD 9-10, K21590, K 21590, 2.25Cr1Mo, A182 F22, A 182 F 22, A182 T22, K21390


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.