1.3207, HS10-4-3-10 - Cobalt high-speed steel according to ISO 4957, DIN 17350.

Standard Steel Grade
Chemical composition %
C: Mn: Si: P: S: Cr: Ni: Mo: V: W: Co:
ISO/DIN HS10-4-3-10 - 1.3207 - S10-4-3-10
1.20 - 1.35 <0.4 <0.45 <0.03 <0.03 3.8 - 4.5 - 3.2 - 3.9 3.0 - 3.5 9.0 - 10.0 9.5 - 10.5
PN SK10V
1.15 - 1.30 <0.4 <0.5 <0.030 <0.030 3.5 - 4.5 <0.4 3.0 - 3.6 2.7 - 3.2 9.0 - 11.0 9.5 - 10.5
GOST R9M4K8 - Р9М4К8
1.0 - 1.1 0.2 - 0.5 0.2 - 0.5 <0.030 <0.030 3.0 - 3.6 <0.6 3.8 - 4.3 2.3 - 2.7 8.5 - 9.5 7.5 - 8.5
ASTM A600 Type M48
1.42 - 1.52 0.15 - 0.40 0.15 - 0.40 <0.03 <0.07 3.5 - 4.0 - 4.75 - 5.50 2.75 - 3.25 9.5 - 10.5 8.0 - 10.0
NF Z130WKCDV10-10-04-04-03
1.20 - 1.35 <0.40 <0.50 <0.030 <0.030 3.5 - 4.5 - 3.0 - 3.5 3.2 - 3.9 9.0 - 10.0 9.5 - 10.5
BS BT42
1.25 - 1.40 <0.40 <0.40 <0.035 <0.035 3.75 - 4.50 <0.4 2.75 - 3.50 2.75 - 3.25 8.5 - 9.5 9.0 - 10.0

 


1.3207, HS10-4-3-10 - specification and application

Tungsten-cobalt-vanadium high-speed steel with very high resistance to abrasion and tempering, high strength at high cutting speeds and hardness above 65 HRC after machining. Steel designed for tools for rough and finishing machining of difficult steels, austenitic stainless steels and materials with high mechanical properties. It has a tendency to decarburize, particularly low impact strength, low ductility, difficult in polishing. Grade used for high-performance milling cutters, planer knives, turning knives, shape knives for automatic machines and peelers.


Mechanical properties of 1.3207, HS10-4-3-10:

  • Softened annealed condition +A: 241-302HB
  • Delivery condition +A+C: <352HB
  • Delivery condition +A+CR: <372HB
  • Hardness after hardening and tempering at temperature:
    • 300C = 61HRC
    • 350C = 61HRC
    • 400C = 62HRC
    • 450C = 64HRC
    • 500C = 66HRC
    • 550C = 67HRC
    • 600C = 65.5HRC
    • 650C = 62HRC
    • 700C = 54.5HRC

Heat treatment - processes and temperatures:

  • Softening annealing at 830-870C for 3-4 hours, cooling with furnace cooling
  • Softening annealing with isothermal transformation at 740C for 4-6 hours with furnace cooling
  • Relief annealing at a temperature of 600-700°C
  • Hardening
    • heating 1 to 580C
    • heating 2 to 900-1000C
    • Heating of simple tools at the temperature of 1220-1230C
    • Heating of complex tools in the temperature of 1200-1210C
    • Cooling in oil or salt bath at 550-570C
  • Air-cooled tempering
    • First tempering at the temperature of 560C
    • Second tempering at the temperature of 530C
  • Nitriding at the temperature of 510-530C

In the above mentioned grades the company delivers:


Other designations of the grade:

S10-4-3-10, R14, JUS C.9683, Z130WKCDV10-10-04-04-03, BT42, SS2736, SKH57, AISI M48, A600 type M48, R9M4K8, Р9М4К8, bohler s700, vk-10e, W10Mo4Cr4V3Co10, CSN 19861, F-5553, Vanadis 30, AISI T42, AISI M48, T11348.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.