Alloy structural steel for nitriding 40CDV12, 40CrMoV13-9, 1.8523, 39CrMoV13 for aviation industry according to EN 10085, AIR 9160C, EN 10250-3.

 

StandardSteel Grade
Chemical Composition %
C:Mn:Si:P:S:Cr:Mo:V:
EN40CrMoV13-9 - 1.8523 - 39CrMoV13
0.36 - 0.430.4 - 0.7<0.4<0.025<0.0353.0 - 3.50.8 - 1.10.15 - 0.25
AIR40CDV12 - 40 CDV 12
0.40.55---3.251.00.2
IS40Cr13Mo10V2
0.35 - 0.450.4 - 0.70.10 - 0.35--3.0 - 3.50.9 - 1.10.15 - 0.25
BS897M39 - 897 M 39 - HCM3
0.35 - 0.430.45 - 0.700.10 - 0.35<0.035<0.0353.0 - 3.50.8 - 1.10.15 - 0.25
BSS132 - S133 - S134
0.40.55---3.251.00.2

 

40CDV12, 40CrMoV13-9, 39CrMoV13, 1.8523 - specifications and application

40CrMoV13-9 / 40CDV12 is a structural alloy steel grade intended for nitriding, of which a similar equivalent with a slightly lower carbon content is 32CDV13 / 33CrMoV12-9 / 1.8522.

The steel is characterized by even greater hardness which reduces surface wear after nitriding, high hardenability, high strength properties, resistance to stress, and higher core plasticity compared to standard nitriding materials. The grade is adapted to the production of components and elements, among others, in the aerospace industry.


Mechanical properties of 40CrMoV13-9, 39CrMoV13, 1.8523, 40CDV12

  • Dimensions 16 - 40mm
    • Tensile strength, Rm: 950 - 1150 MPa
    • The yield point, Re: > 750 MPa
    • Elongation, A:> 11%
    • Impact resistance, KV20℃: >20 J
  • Dimensions 40 - 100mm
    • Tensile strength, Rm: 900 - 1100 MPa
    • The yield point, Re: > 720 MPa
    • Elongation, A:> 13%
    • Impact resistance, KV20℃: >20 J
  • Dimensions 100 - 160mm
    • Tensile strength, Rm: 870 - 1070 MPa
    • The yield point, Re: > 700 MPa
    • Elongation, A:> 14%
    • Impact resistance, KV20℃: >20 J
  • Dimensions 160 - 250mm
    • Tensile strength, Rm: 800 - 1000 MPa
    • The yield point, Re: > 625 MPa
    • Elongation, A:> 15%
    • Impact resistance, KV20℃: >20 J
  • Hardness in +A annealed condition: <248 HB

 


Heat treatment of 40CDV12, 40CrMoV13-9, 1.8523 steel

  • Softening annealing at a temperature of 680 - 720 ℃
  • Hardening at 870 - 970 ℃ with cooling in water or oil (0.5 H at least)
  • Tempering at 580 - 700℃ for a minimum of one hour
  • Nitriding at a temperature of 480 - 570℃

 


In the above mentioned grades, the company offers:

 


Other indications and equivalents of 40CrMoV13-9 steel:

40CrMoV13-9, 39CrMoV13, 1.8523, 40CDV12, FE-PL56, FE-PL1507, 40 CrMoV 13-9, 39 CrMoV 13, 40 CDV 12, 40Cr13Mo10V2, 897M39, 1.8564, 3 S.132, 897 M 39, MSRR 6011, MSRR 6012, MSRR 6097, MSRR 6100, MSRR 6104, MSRR 6119, MSRR 6910, MSRR 6911, MSRR 6912, S132, S133, S134, AMS 6481, GH4, HCM3, E40CDV12.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.