Structural steel for thermal improvement 35NiCr6, 36NiCr6, 1.5710, 1.5815, 35NC6 for heavy-duty part for aviation industry according to EN 10083-3, AIR 9160/C.

 

StandardSteel Grade
Chemical Composition %
C:Mn:Si:P:S:Cr:Ni:Cu:
EN36NiCr6 - 1.5710
0.32 - 0.400.4 - 0.80.15 - 0.35<0.035<0.0350.3 - 0.71.25 - 1.75-
EN/DIN35NiCr6 - 36NiCr6-4 - 1.5815
0.33 - 0.390.6 - 0.90.10 - 0.40<0.035<0.0350.85 - 1.151.20 - 1.60-
DIN40NiCr6 - 1.5711
0.38 - 0.430.7 - 0.90.15 - 0.35<0.035<0.0350.55 - 0.751.1 - 1.4-
AF35NC6
0.33 - 0.390.6 - 0.90.10 - 0.40<0.035<0.0350.85 - 1.151.20 - 1.60-
AF30NC6
0.25 - 0.350.6 - 0.90.10 - 0.40<0.040<0.0350.85 - 1.151.20 - 1.60-
ASTMUNS K22033 - AMS 6330E
0.33 - 0.380.6 - 0.80.20 - 0.35<0.025<0.0250.55 - 0.751.1 - 1.4<0.35

 

35NiCr6, 1.5815, 36NiCr6, 1.5710 - specifications and application

Steel for heat improvement characterized by high strength properties, good ductility, resistance to fatigue and impact. Used for heavy-duty parts of engines, devices and machines, used in the production of crankshafts, gears, shafts, piston rods, bolts, heat-treated gears and piston rods.


Mechanical properties of 35NiCr6, 1.5815, 35NC6 steel in heat-improved condition:

  • Dimensions <16mm
    • Tensile strength, Rm: 880 - 1080 MPa
    • The yield point, Re: > 740 MPa
    • Elongation, A:> 12%
    • Contraction, Z: >40%
  • Dimensions 16 - 40mm
    • Tensile strength, Rm: 880 - 1080 MPa
    • The yield point, Re: > 740 MPa
    • Elongation, A:> 14%
    • Contraction, Z: >40%
    • Impact resistance, KV: > 35J
  • Dimensions 40 - 100mm
    • Tensile strength, Rm: 780 - 980 MPa
    • The yield point, Re: > 640 MPa
    • Elongation, A:> 15%
    • Contraction, Z: >40%
    • Impact resistance, KV: > 35J
  • Hardness in +A annealed condition: <223 HBW

 


Heat treatment:

  • Hardening at 840 - 860 ℃ with cooling in water or oil
  • Tempering at a tempering of 530 - 630℃

 


In the above-mentioned grades we deliver:

 


Other indications of grades and substitutes:

AISI 3140, SNC1, SNC236, 640M40, EN111, 35NC5, 35NC6, 35 NC 6, 30NC6, 30 NC 6, 1.5710, 1.5815, 36NiCr6, 36 NiCr 6, 35NiCr6, 35 NiCr 6, 36 NiCr 6-4, 36NiCr6-4, 35Ni5Cr2, CSN 16240, 40NiCr6, 40 NiCr 6, 1.5711.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.