Alloyed structural boiler steel for nitriding 34CrAlNi7-10, 34CrAlNi7, 1.8550, 1.2891 for work at elevated temperatures.

 

Standard Steel Grade
Chemical Composition %
C: Mn: Si: P: S: Cr: Mo: Ni: Al:
PN 33H2NMJ
0.30 - 0.37 0.4 - 0.6 0.15 - 0.35 <0.025 <0.025 1.5 - 1.8 0.15 - 0.25 0.9 - 1.1 0.8 - 1.1
EN 34CrAlNi7-10 - 1.8550
0.30 - 0.37 0.4 - 0.7 <0.4 <0.025 <0.035 1.5 - 1.8 0.15 - 0.25 0.85 - 1.15 0.8 - 1.2
DIN 34CrAlNi7 - 34 CrAlNi 7 - 1.2891
0.30 - 0.37 0.4 - 0.7 <0.4 <0.025 <0.035 1.5 - 1.8 0.15 - 0.25 0.85 - 1.15 0.8 - 1.2

 

34CrAlNi7-10, 1.8550 - specifications and application

34CrAlNi7 is intended for work at elevated temperatures in an environment that requires high sliding properties, corrosion, temperature, abrasion, and fatigue resistance. Steel with the addition of Nickel and Aluminum used in the energy, machinery, and automotive industries for large cross-sections elements in the heat treated condition. The products are used in the manufacture of screws, rods, cylinders, pistons, gears, extruders, and rings, which do not require welding.


Mechanical properties of 34CrAlNi7-10, 1.8550

  • Dimensions 16 - 40mm
    • Tensile strength, Rm: 900 - 1100 MPa
    • The yield point, Re: > 680 MPa
    • Elongation, A:> 10%
    • Impact resistance, KV20℃: >30J
  • Dimensions 40 - 100mm
    • Tensile strength, Rm: 850 - 1050 MPa
    • The yield point, Re: > 650 MPa
    • Elongation, A:> 12%
    • Impact resistance, KV20℃: >30J
  • Dimensions 100 - 250mm
    • Tensile strength, Rm: 800 - 1000 MPa
    • The yield point, Re: > 600 MPa
    • Elongation, A:> 13%
    • Impact resistance, KV20℃: >35J
  • Hardness in +A condition: <248 HB
  • Hardness of nitrided surface, HV1: 950

 


Heat treatment of 34CrAlNi7-10, 1.8550:

  • Softening annealing at a temperature of 650 - 700 ℃
  • Hardening at 870 - 930 ℃ for at least half an hour with cooling in water or oil
  • Tempering at 580 - 700℃ for a minimum of 700 hour
  • Nitriding at a temperature of 480 - 570℃

 


In the above mentioned grades the company provides:

 


Other grades designations:

33H2NMJ, 1.8550, 34CrAlNi7, 34CrAlNi7-10, 1.2891, 34 CrAlNi 7, 34 CrAlNi 7-10.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.