1.7027, 20Cr4, 5120, 20Ch – case-hardening steel according to ISO 683-17:2014 i GOST 4543-71.

Standard Grade
Chemical composition %
C: Si: Mn: P: S: Cr: Ni: Cu:
PN 20H
0.17-0.23 0.17-0.37 0.5-0.8 <0.035 <0.035 0.7-1.0 <0.3 -
ISO 1.7027
0.17-0.23 <0.4 0.6-0.9 <0.025 <0.030 0.9-1.2 - <0.3
GOST 20Ch - 20H
0.17-0.23 0.17-0.37 0.5-0.8 <0.035 <0.035 0.7-1.0 <0.3 <0.3
ISO 20Cr4
0.17-0.23 0.15-0.40 0.6-0.9 <0.035 <0.035 0.9-1.2 - -
AISI 5120
0.13-0.18 0.15-0.35 0.7-0.9 <0.035 <0.040 0.7-0.9 - -

20H, 1.7027, 20Cr4, 5120, 20Ch – description

Steel used for small parts with higher strength requirements than 15Cr3 steel, e.g. spindles, pins, camshafts and bushings. Weldable, machinable and cuttable steel. Weld only before carburizing.


Physical and mechanical properties

Here You can find the mechanical properties of selected alloys. Despite their similarities, they clearly differ.

Properties Grade
PN ISO GOST ISO
20H 20Cr4 20Ch 1.7027
Yield strength: Rm > 640 MPa > 850 MPa > 637 MPa -
Tensile strength: Rm > 780 MPa 820-1170 MPa > 784 MPa -
Wydłużenie: A5 11 % 9 % 11 % -
Udarność KCU, 20°C: KCU2 J/cm2 60 J/cm2 KU: 25J/cm2 59J/cm2 -
Twardość po odprężaniu: HB < 179 HB < 197 HB < 179 HB < 197 HB

Mechanical properties after hardening:

  • Diameter D: 11 mm
    • Tensile strength Rm: 820-1170 MPa
    • Yield strength Re: min 550 MPa
    • Elongation A: min 9 %
    • Impact Value KU: min 25 J
  • Diameter D: 30 mm
    • Tensile strength Rm: 750-1100 MPa
    • Yield strength Re: min 490 MPa
    • Elongation A: min 9 %
    • Impact Value KU: min 25 J
  • Diameter D: 63 mm
    • Tensile strength Rm: 670-1020 MPa
    • Yield strength Re: min 450 MPa
    • Elongation A: min 10 %
    • Impact Value KU: min 25 J

Heat treatment and plastic working

Following parameters are recommended for working and heat treatment

Treatment Grade
PN ISO GOST ISO
20H 20Cr4 20Ch 1.7027
Quenching Temperature 880℃ 860-900℃ 880℃ 860-900℃
Cooling oil, water - oil, water -
Tempering Temperature 180℃ 150-200℃ 180℃ 150-200℃
Cooling air, oil - air, oil -

We deliver this steel alloy as:

  • Bars, strips and reels
  • Rods
  • Wires
  • Plates

Replacements, equivalents and other designations:

20H, 20Ch, 20Ch-Sh, 20Cr, 1.7027, 20Cr4, SCr22, SCr420, B21, 5120, C41201, 20Ch-PV


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.