Stainless duplex steel 1.4460, AISI 329 resistant to chlorine according to PN-EN 10088-1.

Standards Steel Grades
Chemical Composition %
C: Mn: Si: P: S: Cr: Mo: Ni: N:
EN / DIN X3CrNiMoN27-5-2 - 1.4460
<0.05 <2.0 <1.00 <0.035 <0.030 25.0 - 28.0 1.30 - 2.00 4.5 - 6.5 0.05 - 0.20
AFNOR Z5CND27-05 Az
<0.05 <2.0 <0.75 <0.035 <0.025 26.0 - 27.0 1.30 - 2.00 4.5 - 5.0 0.05 - 0.20

ASTM

AISI 329 - S32900 - Alloy 7Mo
<0.08 <1.0 <0.75 <0.040 <0.030 23.0 - 28.0 1.00 - 2.00 2.5 - 5.0 -
ASTM S31200 - 44LN - Grade F50
<0.03 <2.0 <1.00 <0.045 <0.030 24.0 - 26.0 1.20 - 2.00 5.5 - 6.5 0.14 - 0.20
ASTM J93371 - 25Cr-5Ni-Mo-N - CD6MN - A 781 Grade 3A
<0.06 <1.0 <1.00 <0.040 <0.040 24.0 - 27.0 1.75 - 2.50 4.0 - 6.0 0.15 - 0.25
UNE X8CrNiMo26-6 - F-3552
<0.10 <2.0 <1.00 <0.045 <0.030 24.0 - 27.0 1.30 - 1.80 4.5 - 7.0 <0.10
UNE X8CrNiMo27-05 - F-3309
<0.10 <2.0 <1.00 <0.045 <0.030 26.0 - 28.0 1.30 - 2.00 4.0 - 5.0 -
SS 2324 - SS2324
<0.10 <2.0 <1.00 <0.045 <0.030 24.0 - 27.0 1.30 - 1.80 4.5 - 7.0 -

 

Description and specification

Stainless duplex low-carbon steel resistant to intercrystalline corrosion, fatigue corrosion, crevice corrosion, pitting and stress corrosion. It exhibits excellent resistance to chlorides and, in addition, is susceptible to mechanical processing. It is characterized by high strength, hardness and good plasticity. Commonly used as steel for bearings in chlorine-containing environments.

However, in high temperatures of 300 - 900 ℃, the steel exhibits brittleness. With respect to duplex 1.4462 steel, the described grade has slightly worse corrosion resistance. Duplex 1.4460 steel products are used in the chemical, cryogenic, paper and aviation industries.

X3CrNiMoN27-5-2 steel is designed, among others, for pumps, screws, heat exchangers for power engineering, radiators, tanks, chlorine-bearing housings, valves, air constructions, pipelines, special anchors, pump shafts, stirrers and sleeves. In addition, the steel retains the resistance to intercrystalline corrosion after welding and in the delivery condition.


Mechanical and physical properties

  • Tensile strength: Rm = 620 - 880 MPa
  • Yield point: Re = > 460 MPa
  • Hardness < 260 HB
  • Elongation: A = > 20%
  • Modulus of elasticity, E = 200 GPa
  • Heat conductivity λ = 15 W ⋅ m-1 ⋅ K-1
  • Heat capacity cp20℃ = 500 J ⋅ kg-1 ⋅ K-1
  • Density: ρ = 7,80 kg/dm³

Properties for individual temperatures

Properties Temperatures
100℃ 200℃ 300℃ 400℃ 500℃
Yield point Rp0,2 > 360 MPa > 310 MPa - - -
Linear Expansion Factor α 13.0⋅10-6⋅K-1 13.5⋅10-6⋅K-1 14.0⋅10-6⋅K-1 - -
Modulus of elasticity E 194 GPa 186 GPa 180 GPa - -

In duplex the company 1.4460 supplies:


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.