Chemical composition %
C: Si: Mn: Cr: Mo: V:
DIN 1.2990 / X100CrMoV8-1-1
1.0 0.9 0.8 8.0 1.6 1.6

1.2990 / X100CrMoV8-1-1 – description

Cold-working ledeburitic tool steel for punches, dies, progressive dies, cold rolls, woodworking tools, rotary cutters and rotary shear blades. Strong, hard and hardenable.


Physical and mechanical properties

The hardness after soft annealing: max 250 HBW.

The hardness after toughening depends on the tempering temperature:

  • Tempering temperature: 100 °C - 62-64 HRC
  • Tempering temperature: 200 °C - 59 HRC
  • Tempering temperature: 300 °C - 57-59 HRC
  • Tempering temperature: 400 °C - 58-60 HRC
  • Tempering temperature: 500 °C - 60-63 HRC
  • Tempering temperature: 500 °C - 60-63 HRC
  • Tempering temperature: 525 °C - 60-63 HRC
  • Tempering temperature: 550 °C - 59-61 HRC
  • Tempering temperature: 575 °C - 55-57 HRC
  • Tempering temperature: 600 °C - 46-48 HRC

Thermal conductivity:

  • Testing temperature: 25 °C - 34,2 W/(m*K)
  • Testing temperature: 100 °C - 25,9 W/(m*K)
  • Testing temperature: 150 °C - 26,8 W/(m*K)
  • Testing temperature: 200 °C - 27,1 W/(m*K)
  • Testing temperature: 300 °C - 27,4 W/(m*K)
  • Testing temperature: 400 °C - 27,2 W/(m*K)
  • Testing temperature: 500 °C - 26,8 W/(m*K)

Coefficient of thermal expansion:

  • Temperature range: 20-100 °C - 11,4 10-6*m/(m*K)
  • Temperature range: 20-150 °C - 11,6 10-6*m/(m*K)
  • Temperature range: 20-200 °C - 11,7 10-6*m/(m*K)
  • Temperature range: 20-250 °C - 11,9 10-6*m/(m*K)
  • Temperature range: 20-300 °C - 12,0 10-6*m/(m*K)
  • Temperature range: 20-350 °C - 12,1 10-6*m/(m*K)
  • Temperature range: 20-400 °C - 12,3 10-6*m/(m*K)
  • Temperature range: 20-450 °C - 12,4 10-6*m/(m*K)
  • Temperature range: 20-500 °C - 12,6 10-6*m/(m*K)

Heat treatment and working

Recommended working and heat treatment parameters for 1.2990 alloy:

  • Soft annealing: 830-860 °C
  • Quenching: 1030-1080 °C
  • Stress relieving: 630-670 °C

We deliver this steel alloy as:

  • Bars, flat bars, squares
  • Forgings and forged blocks

Replacements, equivalents and other designations:

1.2990, Thyrodur 2990, X100CrMoV8-1-1


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.