X40CrSiMo10-2, 1.4731, H10S2M - Silchrom valve steel, chromium-silicon, with the addition of molybdenum for valves of internal combustion engines according to PN-71/H-86022 and EN 10090.

 

StandardSteel grade
Chemical Composition %
C:Mn:Si:P:S:Cr:Mo:Ni:V:Ti:W:Cu:
PNH10S2M
0.35 - 0.45<0.71.9 - 2.6<0.035<0.0309.0 - 10.50.7 - 0.9<0.5<0.20-<0.50-
ENX40CrSiMo10-2 - X40CrSiMo10 - X 40 CrSiMo 10-2 - 1.4731 - 4731
0.35 - 0.45<0.82.0 - 3.0<0.040<0.0309.5 - 11.50.8 - 1.3<0.5----
UNEF-3221 - X 40 CrSiMo 10-02 - F3221
0.35 - 0.45<0.82.0 - 3.0<0.040<0.0309.0 - 11.00.8 - 1.3-----
AFNORZ40CSD10 - Z 40 CSD 10
0.35 - 0.45<0.82.0 - 3.0<0.040<0.0309.5 - 11.50.8 - 1.3<0.5----
-4Ch10S2M - 4Х10С2М - 4Kh10S2M - 4H10S2M
0.35 - 0.45<0.81.9 - 3.0<0.030<0.0309.0 - 10.50.7 - 1.2-----
GOST40Ch10S2M - 40Kh10S2M - 40H10S2M - 40Х10С2М - ЭЛ 107 - EL 107
0.35 - 0.45<0.81.9 - 3.0<0.030<0.0259.0 - 10.50.7 - 0.9<0.6<0.20<0.20<0.20<0.30
GB/T4Cr10Si2Mo - S48140
0.35 - 0.45<0.71.9 - 2.6<0.035<0.0309.0 - 10.50.7 - 0.9<0.6----
MSZ 5776SZ4 - SZ 4
0.35 - 0.450.3 - 0.62.4 - 3.0<0.010<0.0309.0 - 10.50.8 - 1.2<0.6---<0.30

 


X40CrSiMo10-2, 1.4731 - specifications and application

H10S2M special valve steel with pearlitic-martensitic structure - heat-resistant up to 900 ℃, and creep-resistant up to approx. 700 ℃.

Mainly used for heavily loaded exhaust valves and loaded inlet valves for aviation, car and motorcycle engines.

The addition of Molybdenum - Mn in relation to H9S2 steel, improves the strength properties, and increases the temperature of resistance to oxidation by 50 ℃.

H10S2M steel is generally not welded.


Mechanical properties of H10S2M

Mechanical and physical properties at normal temperature
Tensile strength, Rm≥ 930 MPa
The yield point, Rp0.2≥ 740 MPa
Elongation A≥ 10 %
Density, ρ~7,72 kg/dm3
Electrical resistance0.90 om mm2/m
Specific heat at 20 °C0.11 cal/g

 


Linear expansion coefficient in the temperature range for H10S2M

Linear expansion coefficient α
20 - 100℃10 ⋅10⁻⁶ K⁻¹
20 - 400℃12.0 ⋅10⁻⁶ K⁻¹
20 - 500℃12.6 ⋅10⁻⁶ K⁻¹
20 - 600℃12.9 ⋅10⁻⁶ K⁻¹
20 - 700℃13.0 ⋅10⁻⁶ K⁻¹
20 - 800℃13.4 ⋅10⁻⁶ K⁻¹

 


Exemplary strength properties at elevated temperature for H10S2M material

- Steel hardened at a temperature of 1025 ℃ in oil and tempered at 800 ℃

TemperatureShort-term tensile test and impact strength testTime creep limitModulus of elasticity, E kG/mm2
Rr (kG/mm2)a5 (%)U (kGm/cm2)R1/10000
20℃----22000
500℃67--22-
600℃35 - 4215.817.52-
700℃15 - 2227.627.50.25-
800℃8 - 1231.237.5--
900℃~54837.5--

 

Thermal conductivity:

  • at a temperature of 20 °C - 0.04 cal/cm sec °C
  • at a temperature of 600 °C - 0.05 cal/cm sec °C

 


Heat treatment of X40CrSiMo10-2

H10S2M chromium-silicon steel with the addition of molybdenum is hardened and tempered with cooling in water or air.

After heat treatment, steel acquires tempered martensite structures.

In poor machining, steel is exposed to temper brittleness.

Heat treatment - process and temperature
Softening annealing at900℃
Hardeningin air or water1010 - 1050℃
Tempering atin oil720 - 780℃

 


In the grade of H10S2M the company provides:

 


The list of equivalents and other designations of H10S2M steel:

X40CrSiMo10-2, X40CrSiMo10, X 40 CrSiMo 10-2, 1.4731, 4731, F-3221, X 40 CrSiMo 10-02, F3221, Z40CSD10, Z 40 CSD 10, 4Ch10S2M, 4Х10С2М, 4Kh10S2M, 4H10S2M, 40Ch10S2M, 40Kh10S2M, 40H10S2M, 40Х10С2М, ЭЛ 107, EL 107, 4Cr10Si2Mo, S48140, SZ4, SZ 4


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.