X30WCrV9-3, 1.2581 - Tool steel for hot work with high content of tungsten according to PN-86/H-85021, and ISO 4957.

 

Standard Steel Grade
Chemical Composition %
C: Mn: Si: P: S: Cr: Ni: V: Mo: W: Sn: Cu:
PN WWV
0.25 - 0.35 0.25 - 0.50 0.15 - 0.50 <0.03 <0.03 2.50 - 3.00 - 0.30 - 0.50 - 8.00 - 10.00 - -
GOST 3Ch2V8F - 3Kh2V8F - 3Х2В8Ф
0.30 - 0.40 0.15 - 0.40 0.15 - 0.40 <0.03 <0.03 2.20 -2.70 <0.35 0.20 - 0.50 - 7.50 - 8.50 - <0.3
BDS 3Ch2B8F
0.30 - 0.40 0.15 - 0.40 0.15 - 0.40 <0.03 <0.03 2.20 - 2.70 <0.35 0.20 - 0.50 - 7.50 - 9.00 - <0.3
EN ISO
4957
X30WCrV9-3 - X 30 WCrV 9-3 - 1.2581 - 2581
0.25 - 0.35 0.15 - 0.45 0.10 - 0.40 <0.03 <0.02 2.50 - 3.20 - 0.30 - 0.50 - 8.50 - 9.50 - -
AFNOR Z 30 WCV 9 - Z30WCV9 - X 30 WCrV 9
0.25 - 0.32 0.15 - 0.45 0.10 - 0.40 - - 2.50 - 3.50 - 0.30 - 0.50 - 8.50 - 9.50 - -
BS BH 21 - BH21 - H 21 - H21
0.25 - 0.35 <0.40 <0.40 - - 2.25 - 3.25 <0.40 <0.40 <0.60 8.50 - 10.0 <0.05 <0.2
ČSN / STN ČSN 19721 - ČSN 19 721
0.25 - 0.35 0.20 - 0.50 0.15 - 0.45 <0.03 <0.03 2.10 - 2.60 - 0.15 - 0.30 - 8.50 - 10.0 - -
ČSN / STN ČSN 19 723 - ČSN 19723
0.20 - 0.30 0.30 - 0.60 0.15 - 0.45 <0.03 <0.03 2.10 - 2.60 1.2 - 1.8 0.05 - 0.15 - 8.50 - 10.0 - -
JIS SKD 5 - SKD5 - SKD 5 M - SKD5M
0.25 - 0.35 0.15 - 0.45 0.10 - 0.40 <0.03 <0.02 2.50 - 3.20 - 0.30 - 0.50 - 8.50 - 9.50 - -
GB/T 3Cr2W8V
0.30 - 0.40 <0.40 <0.40 <0.03 <0.03 2.20 - 2.70 - 0.20 - 0.50 - 7.50 - 9.00 - <0.3
UNI X 30 WCrV 9 3 KU - X30WCrV93KU
0.25 - 0.35 0.15 - 0.45 0.10 - 0.40 - - 2.20 - 3.50 - 0.30 - 0.50 - 8.10 - 9.50 - -

 

X30WCrV9, 1.2581 steel - Specification and application

Tool steel for hot work with high strength and impact resistance when operating at elevated temperatures. It is characterized by high hardenability and high resistance to tempering. The steel exhibits its mechanical properties only at elevated operating temperatures, therefore it is necessary to heat the finished product in the form of tools before use to a temperature of approx. 300℃ WWV steel is also characterized by low thermal conductivity, which makes it unacceptable to quickly cool the element during operation.

X30WCrV9, 1.2581 steel is used as:

  • Steel for high-load dies for making bolts, nuts and rivets
  • Steel for presses for extruding rods
  • Steel for inserts for dies and stamps
  • Steel for extrusion tools
  • Steel on matrices for extrusion of copper alloys
  • Steel for knives for hot-working scissors
  • Steel on the dies for pressing and forging hot brass and bronze
  • Steel for casting molds under pressure of bronze, brass, new silver, magnesium alloys and aluminum
  • Steel for punches
  • Steel for jaws for thread rolling
  • Steel for dies and pins for pulling hot pipes

 


Mechanical properties at different tempering temperatures

Mechanical and physical properties
Processes temperature of tempering Hardness
Softening annealing - ≤ 269 HB
Heat treatment 550℃ ≥ 46 HRC
Hardening - 50 HRC
Hardening and tempering 300℃ 49.5 HRC
350℃ 49.2 HRC
400℃ 48.8 HRC
450℃ 49 HRC
500℃ 49.9 HRC
550℃ 51 HRC
600℃ 48.3 HRC

 


Heat treatment and physical properties

Heat treatment and other properties of WWV steel
Softening annealing in furnace up to 550 ℃ and then 740 - 780℃
Relief annealing slow in the furnace, ash, in the sand 600 - 700℃
Hardening in oil, in the air, in compressed air,
or in a salt bath at 450 - 550 ℃
1120 - 1160℃
Tempering at in air 500 - 600℃
Nitriding 470 - 550℃
Density, ρ ~8.40 kg/dm³
Thermal conductivity λ20℃ 30 W ⋅ m⁻¹ K⁻¹
Coefficient of linear expansion α20-100 ℃ 12.4 ⋅12.4⁻⁶ K⁻¹
Modulus of longitudinal elasticity E 21000 kG/mm2
Transverse modulus of elasticity G 8100 kG/mm3

 


Coefficient of linear expansion, specific heat and electrical resistance

Coefficient of linear expansion: α ⋅ 10° at specified temperatures ℃
20 - 100 0 - 50 0 - 100 0 - 200 0 - 300 0 - 400 0 - 500 0 - 600 0 - 700 0 - 750 0 - 800
- 14.3 K⁻¹ 14.7 K⁻¹ 15.6 K⁻¹ 16.3 K⁻¹ 16.1 K⁻¹ 15.2 K⁻¹ 15.0 K⁻¹ 12.5 K⁻¹ 9.9 K⁻¹ 7.5 K⁻¹
The specific heat cp cal/(g ⋅ ℃)
20℃ 81℃ 241℃ 537℃ 756℃ 900℃
- 0.112 0.125 0.164 0.302 0.158
Specific resistance
ρ ⋅ 104 ⋅ Ω ⋅ cm 30 - 100℃ 200 - 400℃ 400 - 600℃ 600 - 800℃  800 - 1000℃
0.513 (43℃) 0.615 (226℃) 0.813 (464℃) 1.000 (706℃) 1.170 (854℃)
0.520 (78℃) 0.625 (238℃) - - 1.082 (749℃) 1.205 (892℃)

 


In the above mentioned grades, the company offers:

 


The list of equivalents and other designations of WWV:

3Ch2V8F, 3Kh2V8F, 3Х2В8Ф, 3Ch2B8F, X30WCrV9-3, X 30 WCrV 9-3, 1.2581, 2581, Z 30 WCV 9, Z30WCV9, X 30 WCrV 9, BH 21, BH21, H 21, H21, ČSN 19721, ČSN 19 721, ČSN 19 723, ČSN 19723, SKD 5, SKD5, SKD 5 M, SKD5M, 3Cr2W8V, X 30 WCrV 9 3 KU, X30WCrV93KU


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.