X22CrMoV12-1, 1.4923, St12T high temperature boiler steel - designed for high temperature applications up to 600 ℃ for turbine blade forgings according to EN 10302 and EN 10269.

 

Standards Steel Grades
Chemical Composition %
C: Mn: Si: P: S: Cr: Mo: Ni: V: Nb W N:
PN 23H12MNF
0.20 - 0.26 0.3 - 0.8 0.1 - 0.5 <0.035 <0.035 11.0 - 12.5 0.8 - 1.2 0.3 - 0.8 0.25 - 0.35 <0.05 <0.6 -
EN X22CrMoV12-1 - X22CrMoV12.1 - 1.4923
0.18 - 0.24 0.4 - 0.9 <0.5 <0.025 <0.015 11.0 - 12.5 0.8 - 1.2 0.3 - 0.8 0.25 - 0.35 - - -
AFNOR Z 20 CDNbV 11 - Z20CDNbV11
0.18 - 0.25 0.3 - 0.8 0.1 - 0.5 <0.025 <0.015 10.0 - 12.0 0.5 - 1.0 <1.0 0.1 - 0.3 0.25 - 0.55 - 0.05 - 0.10
ČSN
STN
ČSN 17134 - ČSN 17 134
0.17 - 0.23 0.5 - 1.0 0.25 - 0.60 <0.035 <0.030 10.0 - 12.5 0.8 - 1.2 0.3 - 0.8 0.20 - 0.35 - - -
BS BS 762
0.17 - 0.23 <1.0 <0.5 <0.030 <0.030 10.0 - 12.5 0.8 - 1.2 0.3 - 0.8 0.25 - 0.35 - - -
SEW 555 X 21 CrMoV 12-1 - X21CrMoV12-1 - 1.4926
0.20 - 0.26 0.3 - 0.8 <0.5 <0.025 <0.020 11.0 - 12.5 0.8 - 1.2 0.3 - 0.8 0.25 - 0.35 - - -

 

X22CrMoV12-1, 1.4923 - specification and applications

The 23H12MNF high-alloy structural steel is also classified as a heat-resistant steel - it is a martensitic-grade steel dedicated for parts, subassemblies and forgings of blades and parts of steam turbine rotors operating at temperatures up to 600 ℃.

Its application owes to its high resistance to fatigue stress. 23H12MNF also features elements and parts of aircraft construction, components in the chemical, petrochemical and petrochemical industries, as well as parts used in the power industry.

The 23H12MNF is a hard to weld steel.


Mechanical properties of products for individual states of improvement

Mechanical properties X22CrMoV12-1 +QT1 at dimensions below 160mm

  • Tensile strength Rm = 800 - 950 MPa
  • Yield point Re > 600 MPa
  • Elongation A > 14%
  • Contraction Z > 40%
  • Notch toughness KV > 27 J

 

Mechanical properties X22CrMoV12-1 +QT2 at dimensions below 160mm

  • Tensile strength Rm = 900 - 1050 MPa
  • Yield point Re >700 MPa
  • Elongation A > 11%
  • Contraction Z > 35%
  • Notch toughness KV > 20 J

 


The yield point of the X22CrMoV12-1 steel at various temperatures:

  • At a temperature of 300 = Re > 480 MPa
  • At a temperature of 400 = Re > 423 MPa
  • At a temperature of 500 = Re > 343 MPa
  • At a temperature of 600 = Re > 284 MPa

 


In the 1.4923 grade the company provides:

 


List of equivalents and other determinations of 23H12MNF steel:

X22CrMoV12-1, X22CrMoV12, X 12 CrMoV 12-1, 1.4923, 4923, Z20CDNbV11, Z 20 CDNbV 11, BS 762, X21CrMoV12-1, X 21 CrMoV 12-1, 1.4926, 4926, ČSN 17134, ČSN 17 134


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.