High-alloy boiler steel X20CrMoV11-1, 1.4922, 20H12M1F for work at elevated temperatures for pressure applications according to EN 10216-2, EN 10088-1, EN 10302, PN-75/H-84024.

 

Standard Steel Grade
Chemical Composition %
C: Mn: Si: P: S: Cr: Ni: Mo: V: Al: Cu:
EN X20CrMoV11-1 - X20CrMoV12-1 - 1.4922
0.17 - 0.23 <1.0 0.15 - 0.50 <0.025 <0.010 10.0 - 12.5 0.3 - 0.8 0.8 - 1.2 0.25 - 0.35 <0.04 <0.3
PN 20H12MF
0.17 - 0.23 0.3 - 0.8 0.1 - 0.5 <0.035 <0.035 11.0 - 12.5 0.3 - 0.8 0.8 - 1.2 0.25 - 0.35 - -
DIN X20CrMoV12-1 - X 20 CrMoV 12-1
0.17 - 0.23 0.3 - 1.0 <0.4 <0.025 <0.015 10.0 - 12.5 0.3 - 0.8 0.8 - 1.2 0.20 - 0.35 - -
ISO X20CrMoNV11-1-1
0.17 - 0.23 <1.0 0.15 - 0.50 <0.030 <0.030 10.0 - 12.0 0.3 - 0.8 0.8 - 1.2 0.25 - 0.35 <0.02 <0.25
GOST 20Х11МНФ - 20Ch11MNF
0.18 - 0.23 0.3 - 0.8 0.1 - 0.4 <0.030 <0.030 11.0 - 12.5 0.3 - 0.8 0.8 - 1.2 0.25 - 0.35 0.015 - 0.045 -
GOST 20Х12МНФ-Ш - 20Ch12MNF-Sh
0.17 - 0.27 <1.0 <0.5 <0.040 <0.030 12.0 - 14.0 <0.6 0.3 - 1.2 0.25 - 0.35 - -

 

X20CrMoV11-1, 1.4922, 20H12M1F - specification of the grade and application

X20CrMoV11-1, is a similar grade to X22CrMoV12-1, 1.4923 with a martensitic structure in the heat-treated state. Designed for pressure and high temperature applications up to 600 ℃ for devices used mainly in the power, oil and chemical industries.

Steel is mainly supplied in the form of hot-rolled boiler pipes, fittings and sleeves. In contrast to 23H12MNF, the above-mentioned grades shows much better and more stable strength properties in the normalized and tempered +NT conditions.

Steel can be classified as one of the heat-resistant grades.


Mechanical properties of X20CrMoV11-1, 1.4922 acc. to EN 10216-2 in +NT condition

  • Tensile strength, Rm: 690 - 840 MPa
  • The yield point, Rp0,2: >490 MPa
  • Properties of samples tested longitudinally:
    • Elongation, A:> 17%
    • Impact resistance, KV20℃: > 20 J
  • Properties of samples tested transversally:
    • Elongation, A:> 14%
    • Impact resistance, KV20℃: > 20 J

 


Mechanical properties of tubes at elevated temperatures acc. to EN 10216-2 - the yield point

  • Temperature 200℃ - Rp0,2: >430 MPa
  • Temperature 250-205℃ - Rp0,2: >415 MPa
  • Temperature 300℃ - Rp0,2: >390 MPa
  • Temperature 350℃ - Rp0,2: >380 MPa
  • Temperature 400℃ - Rp0,2: >360 MPa
  • Temperature 450℃ - Rp0,2: >330 MPa
  • Temperature 500℃ - Rp0,2: >290 MPa
  • Temperature 550℃ - Rp0,2: >250 MPa

 


In the above mentioned grades the company provides:

 


Other indications and equivalents:

20H12M1F, X20CrMoV11-1, X20CrMoV12-1, X 20 CrMoV 11-1, X 20CrMoV 12-1, 1.4923, BS 762, 20Х12МНФ-Ш - 20Ch12MNF-Sh, 20Х11МНФ - 20Ch11MNF, CSN 422916, 12Cr10MoVNi70.47, X20CrMoNV11-1-1, X20CrMoNi12-01, X 20 CrMoNi 12 01, 20VNiMoCr120, 20 VNiMoCr 120.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.