Acid-resistant stainless steel X8CrNi25-21, X12CrNi25-21, 1.4845, AISI 310S for heavy duty parts working in corrosive environment and temperature up to 1050 ℃ according to EN 10095, SEW 470.

 

Standard Steel Grade
Chemical Composition %
C: Mn: Si: P: S: Cr: Ni: Mo: V: W: N:
PN H23N18
<0.2 <1.5 <1.0 <0.045 <0.030 22.0 - 25.0 17.0 - 20.0 <0.5 <0.2 <0.5 -
EN X8CrNi25-21 - X 8 CrNi 25-21 - 1.4845
<0.1 <2.0 <1.5 <0.045 <0.015 24.0 - 26.0 19.0 - 22.0 - - - <0.11
SEW X12CrNi25-21 - X 12 CrNi 25-21 - 1.4845 - 4845
<0.1 <2.0 <1.5 <0.045 <0.015 24.0 - 26.0 19.0 - 22.0 - - - <0.11
DIN X16CrNi25-20 - X 16 CrNi 25-20 - 1.4843
<0.2 <2.0 1.5 - 2.5 <0.045 <0.030 22.0 - 25.0 19.0 - 22.0 - - - -
GOST 20Ch23N18 - 20Kh23N18 - 20Х23Н18
<0.2 <2.0 <1.0 <0.035 <0.020 22.0 - 25.0 17.0 - 20.0 <0.3 <0.2 <0.2 -
GOST 10Ch23N18 - 10Kh23N18 - 10Х23Н18
<1.0 <2.0 <1.0 <0.035 <0.020 22.0 - 25.0 17.0 - 20.0 <0.3 <0.2 <0.2 -
AFNOR AF Z12CN25-20 - Z 12 CN 25-20
<0.15 <2.0 <1.0 <0.040 <0.030 23.0 - 26.0 18.0 - 21.0 - - - -
ASTM AISI 310S - AISI 310 S - UNS S31008
<0.08 <2.0 <1.5 <0.045 <0.030 24.0 - 26.0 19.0 - 22.0 - - - -
BS 310S24 - 310 S 24
<0.15 <2.0 <1.0 <0.045 <0.030 23.0 - 26.0 19.0 - 22.0 - - - -

 

X8CrNi25-21, 1.4845, AISI 310S - specification and application

Creep-resistant and heat-resistant H23N18 steel is a chromium-nickel austenitic grade with an increased nickel content compared to H23N13, showing high strength, ductility, resistance in air and oxidizing atmosphere to high temperatures up to 1050 ℃. The steel is used for mechanically loaded parts that work at high temperatures.

For H23N18 not every work environment is right. Steel in contact with reducing gases, and containing sulfur compounds in higher concentrations, endures temperatures up to 900 ℃. With small impurities it can work up to 1000 ℃. It is used for parts of the furnace, installations, hooks, stands, trolleys, responsible screws, furnace casings, etc.

Classification of the grade as heat-resistant does not limit the use of forged and rolled products only to work at high temperatures. Many users purchase H23N18, heat-resistant materials, because they are ideal as acid-resistant steel. It is used for parts of furnaces, crucibles, parts of chemical apparatus for gas pyrolysis, hydrogenation or methane convergence. Heat resistance and acid resistance in many cases are used when the components work together.

Products made of H23N18 are usually arc welded using ES-24-18 electrodes. Bending of hot elements from sheets should be carried out at a temperature of 900 - 950 ℃.


Mechanical properties of X8CrNi25-21, X12CrNi25-21, 1.4845, AISI 310S

  • Tensile strength, Rm: 500 - 700 MPa
  • The yield point, Re: > 210 MPa
  • Elongation, A: >33%
  • Modulus of elasticity, E = 196 GPa
  • Thermal capacity, cp20-100: 500 J/kg * K
  • Linear expansion coefficient, 15,0 * 10-6 * K-1
  • Thermal conductivity: 14,7 W/m * K
  • Hardness: < 192 HB

 


Creep limit and creep resistance of 1.4845, X8CrNi25-21 steel:

Properties (MPa) Temperature
600℃ 700℃ 800℃ 900℃
Creep limit R1/1000 100 45 18 10
R1/10000 90 30 10 4
Creep strength Rz/1000 170 80 35 15
Rz/10000 130 40 18 8.5
Rz/100000 80 18 7 3

 


Heat treatment processes:

  • Supersaturation at 1100 - 1150 ℃ in water
  • Rolling and forging at a temperature of 1150 - 950 ℃

 


In the H23N18 grade and equivalents, the company provides:

 


Other replacements and equivalents of the grade:

H23N18, 1.4845, 4845, AISI 310S, AISI 310 S, X6CrNi25-20, 1.4951, 06Cr25Ni20, 0Cr25Ni20, X8CrNi25-21, X12CrNi25-21, CSN 17255, STN 17255, Z12CN25-20, Z 12 CN 25-20, Z12CN26-21, Z 12 CN 26-21, Z8CN25-20, Z 8 CN 25-20, X 12 CrNi 25-21, X12CrNi25-20, X 12 CrNi 25-20, BS 310S24, 310S25, BS 310 S 24, X22CrNi25-20, SUS 310S, 12NiCr250, F-331, 1RE12 WT, 7RE10 AE, 8RE10 R, UNS S31008, UNS S31009, TP310S, AMS 5521, AMS 5572, AMS 5577, AMS 5651, AMS 7490, AISI 310H, TP310H, 20Ch23N18, 20Kh23N18, 20Х23Н18, 10Ch23N18, 10Kh23N18, 10Х23Н18.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.