X6Cr17, 1.4016, AISI 430 - stainless steel
Chromium ferritic stainless steel X6Cr17, 1.4016, AISI 430, H17 according to EN 10088-1.
| Standard | Steel Grade | ||||||||
|---|---|---|---|---|---|---|---|---|---|
| Chemical Composition % | |||||||||
| C: | Mn: | Si: | P: | S: | Cr: | Ni: | |||
| EN | 1.4016 - X6Cr17 | ||||||||
| <0.08 | <1.0 | <1.0 | <0.04 | <0.015 | 16.0 - 18.0 | - | |||
| PN | H17 | ||||||||
| <0.1 | <0.8 | <0.8 | <0.04 | <0.03 | 16.0 - 18.0 | <0.6 | |||
| ASTM | AISI 430 - UNS S43000 | ||||||||
| <0.12 | <1.0 | <1.0 | <0.04 | <0.03 | 16.0 - 18.0 | - | |||
| NF | Z8C17 | ||||||||
| <0.08 | <0.75 | <0.75 | <0.04 | <0.015 | 16.0 - 17.5 | - | |||
| UNI | X8Cr17 | ||||||||
| <0.1 | <1.0 | <0.75 | <0.04 | <0.03 | 16.0 - 18.0 | <0.5 | |||
Specifications and applications of steel
Chromium stainless steel with ferritic structure resistant to basic corrosive environments and to some chemicals in low concentrations.
The steel is resistant to water, steam, alcohols, calcium chloride, nitrates, nitric acid, fats, food products, acetone, benzene, esters, ethers, glycol, glycerine, acids present in food products, adhesives, urea, substances present in the production of fuels and derivatives.
The grade X6Cr17 is not resistant in the environment of hydrochloric acid, hydrofluoric acid, and sulphuric acid.
The grade 1.4016 belongs to the group of economical stainless steels, is not suitable for welding, has lower plasticity and low strength properties. It is used in the oil industry for tanks, fittings, food, textile, automotive, food and household equipment industries.
General mechanical properties of 1.4016 / X6Cr17 +A
- Tensile strength, Rm: 400 - 630 MPa
- Yield strength, Re: >240 MPa
- Elongation, A: >20%
- Modulus of elasticity, E: 220 GPa
- Hardness, HB: <200
- Thermal conductivity, λ: 25 W * m-1 * K-1
- Thermal capacity, cp: 460 J * kg-1 * K-1
- Specific resistance, Ω: 0.6 mkOhm * m
Strength properties at elevated temperatures
| Temperature | 100℃ | 150℃ | 200℃ | 250℃ | 300℃ | 350℃ | 400℃ | |
|---|---|---|---|---|---|---|---|---|
| Yield strength, Rp (MPa) | >220 | >215 | >210 | >205 | >200 | >195 | >190 | |
| Modulus of elasticity, E (GPa) | 215 | - | 210 | - | 205 | - | 195 | |
| Linear expansion coefficient, α (*10-6 K-1) | 10.0 | - | 10.0 | - | 10.5 | - | 10.5 | |
Properties of spring strips 1.4016 / X6Cr17 according to EN 10151
- +C700
- Tensile strength, Rm: 700 - 850 MPa
- Elongation, A: >2%
- +C850
- Tensile strength, Rm: 850 - 1000 MPa
- Elongation, A: >1%
Properties of stainless strips, sheets 1.4016 / X6Cr17 according to EN 10088-4, EN 10088-2 in the condition +A
- Tensile strength, Rm: 450 - 600 MPa
- Yield strength, Rp: >260MPa
- Elongation, A: >20%
Mechanical properties of bars and wires 1.4016 / X6Cr17 according to EN 10088-3, EN 10088-5
- Wires +2D
- diameter 0.05 - 0.1mm - Rm: <950 MPa
- diameter 0.1 - 0.2mm - Rm: <900 MPa
- diameter 0.2 - 1.0mm - Rm: <850 MPa
- diameter 1.0 - 3.0mm - Rm: <800 MPa
- diameter 3.0 - 5.0mm - Rm: <750 MPa
- diameter >5.0mm - Rm: <700 MPa
- +2H wires with diameter >0.05mm
- +C500 - Rm: 500 - 700 MPa
- +C600 - Rm: 600 - 800 MPa
- +C700 - Rm: 700 - 900 MPa
- +C800 - Rm: 800 - 1000 MPa
- +C900 - Rm: 900 - 1100MPa
- Drawn light bars
- dimensions <10mm
- Rm: 500 - 750MPa
- Rp: >320MPa
- A: >8%
- dimensions 10 - 16mm
- Rm: 480 - 750MPa
- Rp: >300 MPa
- A: >8%
- dimensions 16 - 63mm
- Rm: 400 - 700MPa
- Rp: >240 MPa
- A: >15%
- dimensions >63mm
- Rm: 400 - 630 MPa
- Rp: >240MPa
- A: >20%
- dimensions <10mm
Heat treatment processes of steel grade
- Annealing +A at 750 - 850℃
In the above mentioned grades the company provides: