Waspalloy, 2.4654, Haynes® Waspaloy - nickel alloy

Waspalloy, 2.4654, Haynes® Waspaloy - nickel alloy according to ASTM B637, ASME SB637, EN 2582 etc.

Standard Grade
Chemical composition %
Ni: Cr: Co: Mo: Ti: Al: B: Zr: Fe: C: Cu: Si: Mn: P: S: Comments:
ASTM / ASME / UNS Waspalloy / AISI 685 / UNS N07001
Balance 18.0-21.0 12.0-15.0 3.5-5.0 2.8-3.3 1.2-1.4 0.003-0.010 0.02-0.08 <2.0 0.02-0.10 <0.1 <0.15 <0.1 <0.015 <0.008 #
Haynes® International Haynes® Waspaloy
Balance 19.0 13.5 4.3 3.0 1.5 0.006 0.05 <2.0 - <0.1 <0.15 <0.1 - - -
EN 2.4654 / NiCr20Co13Mo4Ti3Al / Ni-P101HT / NiTH1302 / NiP100Ht
Balance 18.0-21.0 12.0-15.0 3.5-5.0 2.8-3.3 1.2-1.4 0.003-0.010 0.02-0.08 <2.0 0.02-0.10 <0.1 <0.15 <0.1 <0.015 <0.008 #
GB/T GH4738 / GH684 / GH738
Balance 18.0-21.0 12.0-15.0 3.5-5.0 2.75-3.25 1.2-1.6 0.003-0.010 0.02-0.08 <2.0 0.03-0.10 <0.1 <0.15 <0.1 <0.015 <0.008 -
ISO NW7001 / NiCr20Co13Mo4Ti3Al
Balance 18.0-21.0 12.0-15.0 3.5-5.0 2.8-3.3 1.2-1.4 0.003-0.010 0.02-0.08 <2.0 0.02-0.10 <0.1 <0.001 <0.1 <0.015 <0.008 #

# - Mg<0.01. Ca<0.01. Pb<0.001. Ag<0.0005. Bi<0.0001

Waspalloy, 2.4654, Waspaloy – description

Waspaloy is a nickel-based, age hardenable superalloy for gas turbine applications. Creep and heat resistant, it is used up to 870°C in the combustion atmospheres. However, in critical, demanding applications, the maximum operating temperature should not exceed 650°C.

Applications

Gas turbine components in aerospace industry - compressor discs, rotor discs, shafts, spacers, seals, rings, casings, fasteners etc.

Physical and mechanical properties

Room temperature physical properties:

  • Density: 8.38 g/cm3
  • Melting temperature: 1330-1360 °C
  • Precipitation temperature: 980 °C

High-temperature Coefficient of thermal expansion, from 20°C to:

  • 500°C: 13.9 μm/m⋅K
  • 600°C: 14.3 μm/m⋅K
  • 700°C: 14.8 μm/m⋅K
  • 800°C: 15.4 μm/m⋅K
  • 900°C: 16.4 μm/m⋅K
  • 1000°C: 17.8 μm/m⋅K

Thermal conductivity:

  • 200°C: 12.6 W/m · K
  • 400°C: 15.7 W/m · K
  • 600°C: 19.1 W/m · K
  • 800°C: 22.7 W/m · K
  • 900°C: 24.5 W/m · K

Tensile modulus:

  • 20°C: 213 GPa
  • 200°C: 204 GPa
  • 400°C: 192 GPa
  • 600°C: 180 GPa
  • 800°C: 164 GPa
  • 1000°C: 146 GPa

Tensile properties Waspalloy after heat treatment according to EN 3220 (see section "Heat treatment" for description):

  • 20°C:
    • Yield strength: >800 MPa
    • Tensile strength: >1210 MPa
    • Elongation: >13 %
    • Reduction of area: >18 %
    • Hardness HV: 350-485
  • 700°C:
    • Long-time strength, 23h: 520 MPa

Rupture stress of Waspaloy alloy after type A heat treatment recommended by Special Metals (see "Heat treatment" section for description):

  • 650°C, 1000h: 615 MPa
  • 705°C, 1000h: 450 MPa
  • 760°C, 1000h: 290 MPa
  • 815°C, 1000h: 180 MPa
  • 870°C, 1000h: 110 MPa

Corrosion behaviour

Good resistance to the corrosion occurring in gas turbines, driven by oxidation, carburisation, and nitridation.

Oxidation - good resistance. 1008h long static oxidation test results:

  • 980°C:
    • Metal loss: 0.0152 mm
    • Average metal affected: 0.079 mm
  • 1095°C:
    • Metal loss: 0.036 mm
    • Average metal affected: 0.14 mm
  • 1150°C:
    • Metal loss: 0.079 mm
    • Average metal affected: 0.33 mm
  • 1205°C:
    • Metal loss: >0.4 mm
    • Average metal affected: >0.4 mm

A sufficient resistance to cyclic oxidation, with heating and cooling periods. According to tests in a flowing air environment at 1095°C with 25-hour cycles, the corrosion rate is 3.15 mm/year. For 168-hour cycles, the rate is 1.19 mm/year.

High-temperature carburisation - very good resistance, as confirmed by carbon absorption in:

  • Ar-5H2-5CO-5CH4 215h; 870°C: 0.3 mg/cm2
  • Ar-5H2-5CO-5CH4 215h; 930°C: 1.3 mg/cm2
  • Ar-5H2-5CO-5CH4 55h; 980­°C: 2 mg/cm2

Weldability

Fair weldability. It weld with relatively little difficulty but sometimes is cracking during required postweld heat treating. To avoid strain-age cracks, the heating rate to the solution annealing temperature should be as fast as possible. Additionally, it is recommended that material to be welded is in solution-treated condition before welding.

Heat treatment, working and machining

Forgeability - good. Hot working range - 1170-980°C.

Solution-treatment and age hardening - various manufacturers and different standards provide slightly different details regarding the recommended heat treatment for the Waspaloy alloy. In each case, however, the process involves solution annealing and multi-stage age hardening.

  • The procedure according to Haynes® International
    • Solution-treatment: 1066-1093°C; rapid air cool / water quench
    • Age hardening I: 996°C; 2h; air cool
    • Age hardening II: 843°C; 4h; air cool
    • Age hardening III: 760°C; 16h; air cool
  • The procedure type A according to Special Metals for optimum high-temperature creep and stress-rupture properties:
    • Solution-treatment: 1080°C; 4h; air cool
    • Stabilizing anneal: 845°C; 24h; air cool
    • Age hardening: 760°C; 16h; air cool
  • The procedure type B according to Special Metals for optimum room- and high-temperature tensile properties:
    • Solution-treatment: 995-1035°C; 4h; oil quench
    • Stabilizing anneal: 845°C; 4h; air cool
    • Age hardening: 760°C; 16h; air cool
  • The procedure according to EN 3220:
    • Solution-treatment: 1010-1080°C; 1h; oil quench
    • Stabilizing anneal: 850°C; 4h; air cool
    • Age hardening: 760°C; 16h; air cool

We deliver this steel alloy as:

  • Rod, bar, wire, forging according to ISO 9723, ISO 9724, ISO 9724, AMS 5704, AMS 5706, AMS 5707, AMS 5708, AMS 5709, AMS 5828, ASTM B 637, ASME SB-637, EN 3220
  • Plates, strips and sheets according to AMS 5544

Substitutes, equivalents and other species designations

Waspalloy
UNS N07001
Waspaloy
Bohler L303
EMVAC WP
Aeralloy Waspalloy
Haynes® Waspaloy
Carpenter Waspaloy
Pyrotool Alloy W
Udimet Waspaloy
Unitemp HS
Unitemp Waspaloy
XEV-H
GH4738
GH684
GH738
2.4654
NiP101HT
Ni-PH1302
Ni-WH1302
Ni-P100HT
Ni-P101HT
NiCr20Co13Mo4Ti3Al
NW7001
AMS 5544
AMS 5586
AMS 5704
AMS 5706
AMS 5707
AMS 5708
AMS 5709
AMS 5828
AISI 685
AMS AS7471
J467 Waspaloy
ASTM N 637 (N07001) / ASME SB-637 (N07001)
ASTM N 637 Grade 685 / ASME SB-637 Grade 685

Need help? Contact us!

Call or send a message, and our representative
will contact you within 24 hours!

We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie preferences
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.