Alloy 690, 2.4642, UNS N06690, Inconel 690 - nickel alloy

Alloy 690, 2.4642, UNS N06690, Inconel® 690 - nickel alloy according to ASTM B 166, EN 10302

Standard Grade
Chemical composition %
Ni: Cr: Fe: Mn: Cu: Si: C: S: P: Comments:
ASTM / UNS Alloy 690 / UNS N06690
>58.0 27.0-31.0 7.0-11.0 <0.5 <0.5 <0.5 <0.05 <0.015 - -
DIN 2.4642
Balance 27.0-31.0 7.0-11.0 <0.5 <0.5 <0.5 <0.05 <0.015 <0.02 Ti<0.5; Al<0.5
ISO NiCr29Fe / NW6690 / NiCr29Fe9
Balance 27.0-31.0 7.0-11.0 <0.5 <0.5 <0.5 <0.05 <0.015 - Co<1.5; Ni:Ni+Co
JIS NCF690
>58.0 27.0-31.0 7.0-11.0 <0.5 <0.4 <0.5 <0.05 <0.015 <0.03 Ni:Ni+Co
YB/T GB/T 0Cr30Ni60Fe10 / H06690 / NS3105 / NS315
>58.0 27.0-31.0 7.0-11.0 <0.5 <0.5 <0.5 <0.05 <0.015 <0.03 Ni:Ni+Co

Alloy 690, 2.4642, Inconel® 690 – description

Alloy 690 is an Ni-Cr-Fe alloy with the highest chromium content (~29%) among nickel alloys suitable for fabrication of pressure equipment. High Cr content gives it exceptional high-temperature oxidizing resistance. Notably, it has good nitridation and sulfidation resistance.

It has more Cr and less C than alloy 600 which makes it more resistant to stress-corrosion cracking in hot high-purity water.

Applications

The alloy is used in applications such as nuclear steam generators, coal gasification, and sulfuric, nitric/hydrofluoric acid processing.

Alloy 690, 2.4642, Inconel® 690 - physical and mechanical properties

Room temperature physical properties:

  • Density: 8.2 g/cm3
  • Specific heat capacity: 450 J/kg⋅K
  • Thermal conductivity: 12 W/m⋅K
  • Linear expansion coefficient: 14.3-17.3 μm/m⋅K
  • Electrical resistivity: 1.15 µΩ⋅m
  • Melting temperature: 1343-1377 °C

High-temperature coefficient of thermal expansion

  • 20-200°C: 14.31 μm/m⋅K
  • 20-300°C: 14.53 μm/m⋅K
  • 20-400°C: 14.80 μm/m⋅K
  • 20-500°C: 15.19 μm/m⋅K
  • 20-600°C: 15.70 μm/m⋅K
  • 20-700°C: 16.18 μm/m⋅K
  • 20-800°C: 16.60 μm/m⋅K
  • 20-900°C: 17.01 μm/m⋅K
  • 20-1000°C: 17.41 μm/m⋅K
  • 20-1000°C: 17.79 μm/m⋅K

High-temperature specific heat:

  • 20°C: 450 J/kg⋅K
  • 200°C: 497 J/kg⋅K
  • 400°C: 551 J/kg⋅K
  • 600°C: 604 J/kg⋅K
  • 800°C: 658 J/kg⋅K
  • 900°C: 684 J/kg⋅K
  • 1000°C: 711 J/kg⋅K
  • 1100°C: 738 J/kg⋅K

High-temperature thermal conductivity:

  • 200°C: 15.4 W/m·K
  • 400°C: 19.1 W/m·K
  • 600°C: 22.9 W/m·K
  • 800°C: 26.6 W/m·K
  • 900°C: 28.5 W/m·K
  • 1000°C: 30.1 W/m·K

High-temperature electrical resistivity:

  • 20°C: 1.148 μΩ·m
  • 200°C: 1.180 μΩ·m
  • 400°C: 1.219 μΩ·m
  • 600°C: 1.239 μΩ·m
  • 800°C: 1.247 μΩ·m
  • 900°C: 1.255 μΩ·m
  • 1000°C: 1.265 μΩ·m

High-temperature Young's modulus (in the annealed condition):

  • 20°C: 206.9 GPa
  • 204°C: 196.5 GPa
  • 316°C: 190.3 GPa
  • 427°C: 183.4 GPa
  • 760°C: 155.1 GPa
  • 980°C: 136.5 GPa
  • 1090°C: 125.5 GPa

Mechanical properties of annealed (+AT) 2.4642 long products according to EN 10302:

  • Yield strength: >240 MPa
  • Tensile strength: >590 MPa
  • Elongation: >30%

High-temperature yield strength of 2.4642 long products, according to EN 10302:

  • 100°C: >236 MPa
  • 200°C: >228 MPa
  • 300°C: >220 MPa
  • 400°C: >216 MPa
  • 500°C: >210 MPa
  • 600°C: >200 MPa
  • 700°C: >156 MPa
  • 800°C: >120 MPa

Temperature stability - Inconel® 690 retains its mechanical properties despite prolonged exposure to high temperatures;

  • Impact strength KV
    • No exposure: 190 J
    • 565°C, 1 000h: 156 J
    • 565°C, 4 000h: 171 J
    • 565°C, 12 000h: 164 J
    • 595°C, 1 000h: 195 J
    • 595°C, 4 000h: 170 J
    • 595°C, 13 428h: 170 J
    • 650°C, 1 000h: 198 J
    • 650°C, 4 000h: 179 J
    • 650°C, 12 000h: 172 J
    • 760°C, 1 000h: 214 J
    • 760°C, 4 000h: 201 J
    • 760°C, 12 000h: 184 J
  • Elongation:
    • No exposure: 48 %
    • 565°C, 1 000h: 45 %
    • 565°C, 4 000h: 45 %
    • 565°C, 12 000h: 44 %
    • 595°C, 1 000h: 45 %
    • 595°C, 4 000h: 43 %
    • 595°C, 13 428h: 44 %
    • 650°C, 1 000h: 46 %
    • 650°C, 4 000h: 54 %
    • 650°C, 12 000h: 41 %
    • 760°C, 1 000h: 44 %
    • 760°C, 4 000h: 44 %
    • 760°C, 12 000h: 46 %

Corrosion behaviour

High-temperature water and dilute aqueous solutions - very good resistance to stress-corrosion cracking in such environments (nuclear steam generator). Superior to alloy 600, alloy X750 and alloy 718.

High-temperature nitridation - excellent resistance to HNO3 and a good resistance to other nitriding agents.

Corrosion rates in nitric-plus-hydrofluoric acid solutions at 60 °C:

  • 10% HNO3 + 3% HF - 0.15mm/year
  • 15% HNO3 + 3% HF - 0.25mm/year
  • 20% HNO3 + 2% HF - 0.15mm/year

High-temperature sulfidation - excellent resistance thanks to the high chromium content.

Corrosion rates in oxidizing and reducing sulfidizing environments at 720 °C:

  • 1,5% H2 + 3%O2 + 36,5% H2 + 59% Ar: 2.3mm/year
  • 1,5% H2S + 98,5% H2: 34.7mm/year

Weldability

Basic data: Weldability group 43 (ISO 15608), brazing P-number 111 (ASME section IX).

Selection of welding consumables:

  • ENiCrFe-3, ENiCrFe-7 (Electrode); ERNiCr-3, ERNiCrFe-7 (Filler metal)
  • Joining with 0-9% Ni steel: ENiCrFe-2 (Electrode); ERNiCr-3 (Filler metal)
  • Joining with copper: ENi-1 (Electrode); ERNi-1 (Filler metal)
  • Joining with Nickel-copper: ENi-1 (Electrode); ERNi-1 (Filler metal)

Precaution is required to minimize copper dilution in the weld, because of the high chromium level of alloy 690. “Buttering” the copper or copper-nickel side of the joint with nickel weld metal prior to welding may be advisable.

Heat treatment, working and machining

Recommended working and heat treatment parameters:

  • Heavy forging: 1230-1040 °C
  • Light forging: >870°C °C
  • Annealing: ~1040 °C

Machining - group C, meaning it's mechanical properties are similar to austenitic stainless steel. It's best machined in cold-drawn or cold-drawn and stress-relieved conditions.

Recommended turning parameters with high-speed steel:

  • Roughing:
    • Feed: 0.25 mm/rev
    • Cutting speed: 15 m/min
  • Finishing:
    • Feed: 0.13 mm/rev
    • Cutting speed: 18 m/min

We deliver this steel alloy as:

  • Condenser and heat exchanger tubes according to ASTM B 163 / ASME SB163
  • Seamless and welded pipes according to ASTM B 167 / ASME SB167. ASTM B 829 / ASME SB829, ISO 6207, EN 10302
  • Plates, strips and sheets according to ASTM B 168 / ASME SB168, ISO 6208
  • Forgings according to ASTM B 564 / ASME SB564

Substitutes, equivalents and other species designations

Alloy 690
N06690
0Cr30Ni60Fe10
H06690
NS3105
NS315
2.4642
NW6690
NiCr29Fe
NCF690
ASTM B 163
ASTM B 166
ASTM B 167
ASTM B 168
ASTM B 516
ASTM B 834
ASME SB163
ASME SB166
ASME SB167
Inconel® 690
Sanicro® 690
Allvac 700
Haynes® 690
Nicrofer® 6030
DMV® 690
VDM® Alloy 690

Need help? Contact us!

Call or send a message, and our representative
will contact you within 24 hours!

We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie preferences
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.