Alloy 601, 2.4851, UNS N06601, Inconel 601 - nickel alloy

Alloy 601, 2.4851, UNS N06601, Inconel® 601 - nickel alloy according to ASTM B166, DIN 17754

Standard Grade
Chemical composition %
Ni: Cr: Fe: Al: Mn: Cu: Si: C: S: P: Comments:
ASTM / UNS Alloy 601 / N06601
58.0-63.0 21.0-25.0 Reszta 1.0-1.7 <1.0 <1.0 <0.5 <0.1 <0.015 - -
EN / DIN 2.4851 / NiCr23Fe
58.0-63.0 21.0-25.0 <18.0 1.0-1.7 <1.0 <0.5 <0.5 0.03-0.10 <0.015 <0.02 Ti<0.5; Co<1.5; B<0.006; Ni:Ni+Co
ISO NW6601 / Ni6601 / SNi6601
58.0-63.0 21.0-25.0 <20.0 1.0-1.7 <1.0 <1.0 <0.5 <0.1 <0.015 <0.03 Co<1.0; ET<0.5; Ni:Ni+Co
ISO NiCr23Fe15Al
58.0-63.0 21.0-25.0 Reszta 1.0-1.7 <1.0 <1.0 <0.5 <0.1 <0.015 - Co<1.5; Ni:Ni+Co
BS BS2901 NA49
58.0-63.0 21.0-25.0 Reszta 1.0-1.7 <1.0 <1.0 <0.5 <0.1 <0.015 <0.03 Co<1.0; Ni:Ni+Co
JIS NCF601
58.0-63.0 21.0-25.0 Reszta 1.0-1.7 <1.0 <1.0 <0.5 <0.1 <0.015 <0.03 Ni:Ni+Co
GB/T H06601 / HNS3103 / NS3103
58.0-63.0 21.0-25.0 Reszta 1.0-1.7 <1.0 <1.0 <0.5 <0.1 <0.015 <0.03 ET<0.5

Aloy 601, Inconel® 601– description

Alloy 601 is a Ni-Cr-Fe alloy with outstanding high-temperature strength and oxidation resistance.

The alloy can be either solution-treated or annealed. In the solution-treated condition, alloy 601 is used for rupture-limited applications above 540°C. Annealing is best for tensile-limited applications below 540°C.

Applications

Alloy 601 is a general-purpose engineering material, used most notably in petrochemical and refining plants in high-temperature oxidizing environments, where requirements are too demanding for Alloy 800H/HT.

Aloy 601, Inconel® 601 - physical and mechanical properties

Room temperature physical properties:

  • Density: 8.1 g/cm3
  • Specific heat capacity: 450 J/kg⋅K
  • Thermal conductivity: 11.3 W/m⋅K
  • Linear expansion coefficient: 14.4-17.7 μm/m⋅K
  • Electrical resistivity: 1.19 µΩ⋅m

Coefficient of thermal expansion and temperature (linear):

  • 20-100°C: 13.75 μm/m⋅K
  • 20-200°C: 14.36 μm/m⋅K
  • 20-300°C: 14.58 μm/m⋅K
  • 20-400°C: 14.83 μm/m⋅K
  • 20-500°C: 15.19 μm/m⋅K
  • 20-600°C: 15.62 μm/m⋅K
  • 20-700°C: 16.11 μm/m⋅K
  • 20-800°C: 16.67 μm/m⋅K
  • 20-900°C: 17.24 μm/m⋅K
  • 20-1000°C: 17.82 μm/m⋅K

Specific heat and temperature:

  • 20°C: 448 J/kg⋅K
  • 200°C: 498 J/kg⋅K
  • 400°C: 548 J/kg⋅K
  • 600°C: 603 J/kg⋅K
  • 800°C: 657 J/kg⋅K
  • 900°C: 686 J/kg⋅K
  • 1000°C: 712 J/kg⋅K

Thermal conductivity and temperature:

  • 20°C: 11.2 W/m·K
  • 200°C: 14.3 W/m·K
  • 400°C: 17.7 W/m·K
  • 600°C: 21.0 W/m·K
  • 800°C: 24.4 W/m·K
  • 900°C: 26.1 W/m·K
  • 1000°C: 27.8 W/m·K

Electrical resistivity and temperature:

  • 20°C: 1.18 μΩ·m
  • 200°C: 1.207 μΩ·m
  • 400°C: 1.229 μΩ·m
  • 600°C: 1.247 μΩ·m
  • 800°C: 1.249 μΩ·m
  • 900°C: 1.259 μΩ·m
  • 1000°C: 1.262 μΩ·m

High temperature dynamic modulus of elasticity and temperature:

  • 20°C: 206.5 GPa
  • 200°C: 196.8 GPa
  • 400°C: 184.8 GPa
  • 600°C: 170.8 GPa
  • 800°C: 150.2 GPa
  • 900°C: 137.9 GPa
  • 1000°C: 124.7 GPa

Mechanical properties of 2.4851 bars according to DIN 17750:

  • Yield strength: >205 MPa
  • Tensile strength: 550-750 MPa
  • Elongation: >30%
  • Hardness HB: <220

Tensile properties of hot-drawn bars of annealed (1090°C) Inconel® 601 bars, according to the manufacturer:

  • Room temperature
    • Yield strength: 290 MPa
    • Tensile strength: 741 MPa
    • Elongation: 47 %
  • 300°C
    • Yield strength: 221 MPa
    • Tensile strength: 674 MPa
    • Elongation: 46 %
  • 500°C
    • Yield strength: 203 MPa
    • Tensile strength: 640 MPa
    • Elongation: 45 %

1000h rupture strength of solution-treated (1150°C) Inconel® 601 sheet:

  • 650°C: 195 MPa
  • 760°C: 60 MPa
  • 870°C: 30 MPa
  • 980°C: 15 MPa

Temperature stability - alloy 601 retains its mechanical properties despite prolonged exposure to high temperatures. This is shown by the KV impact strength after exposure to high temperatures of a rod made of Inconel® 601 alloy (solution-treated for thermal stability).

  • No exposure: 176 J
  • 540°C, 100h: 117 J
  • 540°C, 1000h: 121 J
  • 650°C, 1000h: 127 J
  • 700°C, 100h: 129 J
  • 820°C, 159h: 159 J
  • 870°C, 103h: 159 J

Corrosion behaviour

High-temperature oxidation resistance - exceptional up to 1200°C, thanks to the forming of a protective chromium scale. However, above the temperature of about 1000°C the scale begins to convert into volatile CrC3, which makes a difference in prolonged exposure. Thus for applications where the temperature exceeds 1000°C for extensive periods of time alloy 214 will be a better choice.

Average metal affected after 1008h of static oxidation test at indicated temperatures:

  • 980°C: 0.033 mm
  • 1095°C: 0.067 mm
  • 1150°C: 0.135 mm
  • 1205°C: 0.19 mm

Dynamic oxidation resistance in high-velocity combustion gas stream test results (samples were cycled to less than 260°C once every 30 min):

  • 500h, 1090°C:
    • Metal loss: 0.033 mm
    • Maximum metal affected: 0.067 mm with internal nitrides through thickness
  • 1000h, 980°C
    • Metal loss: 0.076 mm
    • Maximum metal affected: 0.51

Results of a dynamic oxidation field test in a natural gas-fired furnace. The test took 113 days at 1090-1230°C with frequent cycles to 540°C:

  • Metal loss: 0.18 mm
  • Maximum metal affected: 0.067 mm with internal nitrides through thickness

Cycling oxidation resistance test lasting for 504h in air-5H2O at 1100°C:

  • Weight change: -11.0 mg/cm2
  • Maximum metal affected: 0.067 mm with internal nitrides through thickness

High-temperature carburization - good resistance. Carbon absorption after 100h in H2M/sub>-2CH4 at 1000°C equaled 10 mg/cm2.

High-temperature nitridation - good to very good resistance. Alloy 601 is one of the alloys most resistant to high-temperature pure nitrogen and it is very resistant to high-temperature ammonia. Depth of nitride penetration as the results of various nitridation tests are presented below:

  • Ammonia 168 h; 650°C: 0.03 mm
  • Ammonia 168 h; 980°C: 0.17 mm
  • Ammonia 168 h; 1090°C: >0.58 mm
  • Pure nitrogen 168 h; 980°C: 1.55 mm
  • Pure nitrogen 168 h; 1090°C: 2.79 mm
  • Pure nitrogen 168 h; 1204°C: 3.81 mm

High-temperature sulfidation - very poor resistance, due to high nickel content.

High-temperature halogenation - good resistance, which is evident from the weight-loss experienced after the following tests:

  • Ar-30Cl2 500 h; 400°C: 0.3 mg/cm2
  • Ar-30Cl2 500 h; 500°C: 3 mg/cm2
  • Ar-30Cl2 500 h; 600°C: 85-200 mg/cm2
  • Ar-30Cl2 500 h; 705°C: 215 mg/cm2
  • Ar-20O2-0.25Cl2 400 h; 900°C: 20.67 mg/cm2
  • Ar-20O2-0.25Cl2 400 h; 1000°C: 124.99 mg/cm2
  • HCl 300h; 400°C: 1.58 mg/cm2
  • HCl 1000h; 400°C: 1.47 mg/cm2
  • HCl 100h; 500°C: 2.57 mg/cm2
  • HCl 300h; 500°C: 4.14 mg/cm2
  • HCl 1000h; 500°C: 9.38 mg/cm2
  • HCl 100h; 600°C: 9.01 mg/cm2
  • HCl 300h; 600°C: 19.46 mg/cm2
  • HCl 96h; 700°C: 102.5 mg/cm2

Weldability

Basic data: Weldability group 43 (ISO 15608), brazing P-number 111 (ASME section IX).

Selection of welding consumables:

  • ENiCrFe-3, ENiCrMo-3 (Electrode); ERNiCr-3, ERNiCrMo-3 (Filler metal)
  • Joining with stainless steel: ENiCrFe-2 (Electrode); ERNiCr-3 (Filler metal)
  • Joining with low-alloy steel: ENiCrFe-2 (Electrode); ERNiCr-3 (Filler metal)
  • Joining with 5-9% Ni steel: ENiCrFe-2 (Electrode); ERNiCr-3 (Filler metal)
  • Joining with copper: ENi-1 (Electrode); ERNi-1 (Filler metal)
  • Joining with Nickel-copper: ENi-1 (Electrode); ERNi-1 (Filler metal)

Heat treatment, working and machining

The alloy can be hot- and cold-worked and can be either solution-treated (max rupture strength) or annealed (max tensile strength). Recommended working and heat treatment parameters:

  • Hot working: 1200-1000 °C
  • Solution-treatment: 1100-1200 °C
  • Annealing: 1000-1100 °C

During solution treatment or annealing, the piece should be held in the furnace for 30-60 min and then be water quenched or rapid air cooled (continuous annealing) or held for 60-180 min and air-cooled (batch annealing).

Machining - group C, meaning its mechanical properties are similar to austenitic stainless steel. It's best machined in cold-drawn or cold-drawn and stress-relieved conditions.

Recommended turning parameters with high-speed steel:

  • Roughing:
    • Feed: 0.25 mm/rev
    • Cutting speed: 15 m/min
  • Finishing:
    • Feed: 0.13 mm/rev
    • Cutting speed: 18 m/min

Recommended turning parameters with carbides:

  • Roughing:
    • Feed: 0.2 mm/rev
    • Cutting speed: 114 m/min
  • Finishing:
    • Feed: 0.1 mm/rev
    • Cutting speed: 130 m/min

Twist drilling with high-speed steel drills recommended parameters:

  • Drill diameter: 3.2-4.8 mm
  • Feed: 0.05-0.10 mm/rev
  • Cutting speed: 8-11 m/min

We deliver this steel alloy as:

  • Rod, bar, wire, forging according to ASTM B 166 / ASME SB166. DIN 17752. ISO 9723. DIN 17753. ISO 9724. DIN 17754. ISO 9725. EN10095
  • Plates, strips and sheets according to ASTM B 168 / ASME SB168. EN10095
  • Seamless and welded pipes according to ASTM B 167 / ASME SB167. ASTM B 751 / ASME SB751. ASTM B 775 / ASME SB 775. ASTM B 829 / ASME SB 829. DIN 17751. ISO 6207

Substitutes, equivalents and other species designations

Alloy 601
H06601
HNS3103
2.4851
NiCr23Fe
BSNA49
NW6601
Ni6601
NiCr23Fe15Al
SNi6601
NCF601
ASTM B 163
ASTM B 166
ASTM B 167
ASTM B 168
ASTM B 474
ASTM B 516
ASME SB163
ASME SB166
ASME SB167
ASME SB516
EMVAC 601
VAT 601
NY 601
Nicrimphy 601
Coralloy 601
Inconel® 601
NRX 601
GL 5 Valbruna

Need help? Contact us!

Call or send a message, and our representative
will contact you within 24 hours!

We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie preferences
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.