Alloy C-276, 2.4819, UNS N10276 - nickel alloy

Alloy C-276, UNS N10276, 2.4819 - otherwise hastelloy C-276, CrNiMo16-60-16, NiMo16Cr15Fe6W4 according to ASTM B462 and ISO 9722

Standard Grade
Chemical composition %
Ni: Mo: Cr: Fe: W: Co: Mn: V: Si: P: S: C: Comments:
ASTM, UNS C-276, Alloy 276, W80276, Hastelloy C-276
Balance 15.0-17.0 14.5-16.5 4.0-7.0 3.0-4.5 <2.5 <1.0 <0.35 <0.08 <0.03 <0.03 <0.01 <0.01
ISO CrNiMo 15-60-16
Balance 15.0-17.0 14.5-16.5 4.0-7.0 3.0-4.5 <2.5 <1.0 <0.35 <0.08 <0.04 <0.03 <0.01 Ni + Co > 52.0
ISO NiMo16Cr15Fe6W4
Balance 15.0-17.0 14.5-16.5 4.0-7.0 - <2.5 <1.0 <0.35 <0.08 <0.04 <0.03 <0.01 <0.01
DIN 2.4886, 2.4887, Sg-NiMo16Cr16W, EL-NiMo15Cr15W
>50.0 15.0-17.0 14.5-16.5 4.0-7.0 3.0-4.5 <1.0 <1.0 <0.4 <0.08 - <0.015 <0.02 Ni: Ni + Co; ET < 0.5
DIN 2.4537
>52.0 15.0-18.0 14.0-18.0 <7.0 3.0-5.0 - <1.0 - <1.0 <0.045 <0.03 <0.1 Cu: <0.5
GOST 02Ch15N60M16
Balance 15.0-17.0 14.5-16.5 4.0-7.0 - <2.5 <1.0 <0.35 <0.08 <0.04 <0.03 <0.01 Ni: Ni + Co

N10276, Alloy C-276, hastelloy c-276, CrNiMo 16-60-16, NiMo16Cr15Fe6W4 – description

Alloy C-276, known widely as N10276 or Hastelloy C-276 is one of the Nickel-Chronium-Molybdenum alloys, having nickel as the primary element. Like every other alloy in this family, it has exceptional heat and corrosion resistance properties.

History and composition - Alloy C-276 can be seen as an upgrade of Alloy C (N30002) with significantly reduced carbon and silicon content. Alloy C was used in the chemical processing industry for many years, but had to be replaced due to its significant limitations. Alloy C has to be solution treated to remove detrimental weld heat-affected zone (HAZ) precipitates. In oxidizing and chloride-containing environments it could be susceptible to intergranular corrosion, when used in the as-welded condition. Alloy C-276 was made to answer those problems and can be welded without introducing susceptibility to intergranular corrosion. Corrosion behaviour as well as further alterations of this alloy are discussed in further sections of this article.

Applications

Alloy C-276 is used in chemical processing, pollution control, pulp and paper production, industrial and municipal waste treatment, and the recovery of sour natural gas.

Applications include stack liners, ducts, dampers, scrubbers, stack-gas reheaters, fans, fan housings, heat exchangers, reaction vessels, evaporators, and transfer piping.

 

N10276 - physical and mechanical properties

Room temperature physical properties:

  • Density: 8.9 g/cm3
  • Linear expansion coefficient: 11.2 *10-6m/(m*K)
  • Thermal conductivity: 9.8 W/(m*K)
  • Specific heat capacity: 427 J/(kg*K)
  • Young's modulus: 205 GPa
  • Electrical resistivity: 1.3 μΩ*m
  • Superconductor at -73°C (-100°F)
  • Shear modulus: 79 GPa
  • Melting temperature: 2415-2500 °C

Mechanical properties of N10276 / C-276 (solution annealed):

  • Yield strength: > 283 MPa
  • Tensile strength Rm: > 690 MPa
  • Elongation: > 40 %
  • Hardness: 90 HRB

Elastic modulus and temperature (average, in tension)

  • In ambient temperature: 205 GPa
  • 204°C: 195 GPa
  • 316°C: 188 GPa
  • 427°C: 182 GPa
  • 538°C: 176 GPa

Coefficient of thermal expansion and temperature (linear):

  • 24-93°C: 11.2 *10-6m/(m*K)
  • 24-205°C: 12.0 *10-6m/(m*K)
  • 24-315°C: 12.8 *10-6m/(m*K)
  • 24-425°C: 13.2 *10-6m/(m*K)
  • 24-540°C: 13.4 *10-6m/(m*K)
  • 24-650°C: 14.1 *10-6m/(m*K)
  • 24-760°C: 14.9 *10-6m/(m*K)
  • 24-870°C: 15.9 *10-6m/(m*K)
  • 24-925°C: 16.0 *10-6m/(m*K)

Thermal conductivity and temperature:

  • -168°C: 7.2 W/(m*K)
  • -73°C: 8.6 W/(m*K)
  • -18°C: 9.4 W/(m*K)
  • 38°C: 10.2 W/(m*K)
  • 93°C: 11.1 W/(m*K)
  • 205°C: 13.0 W/(m*K)
  • 315°C: 15.0 W/(m*K)
  • 425°C: 16.9 W/(m*K)
  • 540°C: 19.0 W/(m*K)
  • 650°C: 20.9 W/(m*K)
  • 760°C: 23.0 W/(m*K)
  • 870°C: 24.9 W/(m*K)
  • 980°C: 26.7 W/(m*K)
  • 1090°C: 28.2 W/(m*K)

Corrosion behaviour

N10276 has exceptional resistance to severe media, including reducing and oxidizing acids, highly oxidizing neutral and acid chlorides, solvents, formic and acetic acids, acetic anhydride, wet chlorine gas, hypochlorites and chlorine solutions.

Average corrosion rates:

  • Hydrochloric acid HCl. 2%. boiling: 1.09 mm/rok
  • Hydrochloric acid HCl. 3%. 66°C: <0.03 mm/rok
  • Hydrochloric acid HCl. 5%. 66°C: 0.13-0.51 mm/rok
  • Hydrochloric acid HCl. 10%. 66°C: 0.51 mm/rok
  • Hydrochloric acid HCl. 15%. 66°C: 0.7 mm/rok
  • Hydrochloric acid HCl. 15%. 93°C: 1.7 mm/rok
  • Hydrochloric acid HCl. 15%. 121°C: 6.4 mm/rok
  • Sulphuric acid H2SO4. 10%. boiling: 0.51 mm/rok
  • Sulphuric acid H2SO4. 80%. 80°C: 0.58 mm/rok
  • 10% H2SO4 + 2% HCl. wrzące: 3.51 mm/rok
  • Nitric acid HNO3. 10%. wrzący: 0.41 mm/rok
  • Phosphoric acid H3PO4. 30%. boiling: <0.13 mm/rok
  • Phosphoric acid H3PO4. 85%. boiling: 0.13-0.64 mm/rok
  • Acetic acid. 99%. boiling: 0.0076 mm/rok
  • Formic acid. 88%. boiling: 0.03 mm/rok
  • Ferric chloride. 10%. boiling: 0.05 mm/rok

Pitting - N10276 shows very high resistance to pitting in oxidizing chloride environments. The critical pitting temperature in 6% FeCl for 24h equals 60-65°C.

Intergranular corrosion - low carbon and silicon content make C-276 much less susceptible to intergranular corrosion. This means a much slower rate of precipitation in this alloy, compared to those with higher carbon and silicon concentrations. It takes some 30 times longer for Alloy C-276 to develop precipitates, compared to Alloy C.

Hydrogen embrittlement - alloy C-276 resists sulfide stress cracking and stress-corrosion cracking in sour gas environments with hydrogen sulfide, carbon dioxide and chlorides.

Limitations - the corrosion resistance of alloy C-276 is somewhat hampered by the precipitation of an intermetallic compound of tungsten and molybdenum. The alloy is especially susceptible to μ-phase formation when exposed to temperatures ranging from 650 to 1095 °C.

Weldability

Weldability - the alloy belongs to group 43 according to ISO 15608. For brazing, the p-number is equal to 111, according to ASME/AWS.

Selection of welding consumables for Alloy C-276

  • Coated electrodes: ENiCrMo3
  • Filler metals: ERNiCrMo-4 through -10

A nitrogen blanket is important to strengthen the welds. The corrosion rate of welded alloy C-276 in 70% HF equals:

  • Nitrogen blanket: 0.008 mm/year
  • Oxygen blanket: 0.94 mm/year

Heat treatment and working

Recommended working and heat treatment parameters for C-276 alloy:

  • Solution annealing: 1107-1135 °C

We deliver this steel alloy as:

  • Forgings
  • Wires
  • Bars
  • Strips
  • Sheets
  • Plates

Variants of C-276 with different chemical composition, properties and applications:

  • N06455 / Alloy C-4 - improved thermal stability.
  • N06022 / Alloy C-22 - better resistance to chloride-induced localized corrosion and sulfide stress cracking.
  • N06059 / Alloy 59 - better resistance to corrosion
  • C06200 / Alloy C-2000 - improved corrosion resistance in sulfuric acid and reducing media

Substitutes, equivalents and other species designations

C-276
N10276
AL276
Nickelvac C-276
Unitemp HN
Inconel alloy C-276
02Ch15N60M16
EP375
CrNiMo15-60-16
NiMo16Cr15
NiMo16Cr15C
2.4886
SG-NiMo16Cr16W
2.4887
EL-NiMo15Cr15W
NiMo16CrW
2.4537
NA48
NiMo16Cr15Fe6W
DNiCrMo-4
DNiCrMo-5
YNiCrMo-4
Alloy C-276
Bohler L276
VRC 279
HGH3113
NS333
NS334
Ch15N55M16V
Nistelle C-276 Deloro
Hastelloy C-276
Phyweld 276
SY 276
W80276

Need help? Contact us!

Call or send a message, and our representative
will contact you within 24 hours!

We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie preferences
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.