Alloy C-263, 2.4650, Nimonic® alloy 263, Haynes® 263 - nickel alloy

Alloy C-263, 2.4650, UNS N07263, Nimonic® alloy 263, Haynes® 263 - nickel alloy according to DIN 17750, AMS 5886

Standard Grade
Chemical composition %
Ni: Co: Cr: Mo: Ti: C: Al: Mn: Si: S: P: Fe: Cu: Pb: Ag: B: Bi: Al+Ti
ASTM / UNS Alloy C-263 / UNS N07263
Balance 19.0-21.0 19.0-21.0 5.6-6.1 1.9-2.4 0.04-0.08 <0.6 <0.6 <0.4 <0.007 <0.015 <0.7 <0.2 <0.002 <0.0005 <0.005 <0.0001 2.4-2.8
Haynes® Haynes® 263 alloy
Balance 20.0 20.0 6.0 <2.4 <0.06 <0.6 <0.4 <0.2 - - - - - - <0.005 - <2.6
DIN 2.4650 / NiCr20Co18Ti
Balance 19.0-21.0 19.0-21.0 5.6-6.1 1.9-2.4 0.04-0.08 <0.6 <0.6 <0.4 <0.007 <0.015 <0.7 <0.2 <0.002 <0.0005 <0.005 <0.0001 2.4-2.8
BS BS HR10 / HR206 / HR404
Balance 19.0-21.0 19.0-21.0 5.6-6.1 1.9-2.4 0.04-0.08 <0.6 <0.6 <0.4 <0.007 <0.015 <0.7 <0.2 <0.002 <0.0005 <0.005 <0.0001 2.4-2.8
ISO NW7263 / NiCr20Cr20Mo5Ti2Al
Balance 19.0-21.0 19.0-21.0 5.6-6.1 1.9-2.4 0.04-0.08 <0.6 <0.6 <0.4 <0.007 <0.015 <0.7 <0.2 <0.002 <0.0005 <0.005 <0.0001 2.4-2.8

Alloy C-263, 2.4650, UNS N07263, Nimonic® alloy 263 – description

Alloy C-263 (UNS N07263) is a high-temperature, precipitation-hardened, creep-resistant Ni-Cr-Co-Mo alloy. It is supplied in the annealed condition. It is recommended for service temperatures up to 850°C, but it resists oxidation up to 1000°C. It is easily weldable (no susceptibility to post-weld heat treatment cracking), has good fabrication characteristics, good wear resistance, and does not exhibit intermediate temperature tensile ductility.

Applications

Alloy C-276 is used in aero and industrial gas turbines for low-temperature combustion chambers, transition liners, exhaust cones and rings.

Physical and Tensile Properties

Room temperature physical properties:

  • Density: 8.4 g/cm3
  • Melting temperature: 1300-1360 °C
  • Magnetic permeability: <1.001

High-Temperature Coefficient of Thermal Expansion, from 20°C to:

  • 100°C: 10.7 μm/m⋅K
  • 200°C: 12.0 μm/m⋅K
  • 300°C: 12.5 μm/m⋅K
  • 400°C: 13.0 μm/m⋅K
  • 500°C: 13.5 μm/m⋅K
  • 600°C: 14.1 μm/m⋅K
  • 700°C: 14.9 μm/m⋅K
  • 800°C: 15.9 μm/m⋅K
  • 900°C: 17.2 μm/m⋅K
  • 1000°C: 18.2 μm/m⋅K

Thermal Conductivity:

  • 20°C: 11.7 W/m · K
  • 100°C: 13.0 W/m · K
  • 200°C: 14.7 W/m · K
  • 300°C: 16.3 W/m · K
  • 400°C: 18.0 W/m · K
  • 500°C: 19.7 W/m · K
  • 600°C: 21.4 W/m · K
  • 700°C: 23.0 W/m · K
  • 800°C: 24.7 W/m · K
  • 900°C: 26.8 W/m · K
  • 1000°C: 28.5 W/m · K

Electrical Resistivity:

  • 20°C: 1.15 μΩ·m
  • 100°C: 1.17 μΩ·m
  • 200°C: 1.18 μΩ·m
  • 300°C: 1.2 μΩ·m
  • 400°C: 1.22 μΩ·m
  • 500°C: 1.24 μΩ·m
  • 600°C: 1.26 μΩ·m
  • 700°C: 1.26 μΩ·m
  • 800°C: 1.25 μΩ·m
  • 900°C: 1.24 μΩ·m
  • 1000°C: 1.24 μΩ·m

Specific Heat Capacity:

  • 20°C: 426 J/kg⋅K
  • 100°C: 447 J/kg⋅K
  • 200°C: 472 J/kg⋅K
  • 300°C: 497 J/kg⋅K
  • 400°C: 523 J/kg⋅K
  • 500°C: 548 J/kg⋅K
  • 600°C: 573 J/kg⋅K
  • 700°C: 598 J/kg⋅K
  • 800°C: 624 J/kg⋅K
  • 900°C: 649 J/kg⋅K
  • 1000°C: 674 J/kg⋅K

Young's Modulus:

  • 20°C: 222 GPa
  • 100°C: 218 GPa
  • 200°C: 212 GPa
  • 300°C: 206 GPa
  • 400°C: 198 GPa
  • 500°C: 192 GPa
  • 600°C: 184 GPa
  • 700°C: 176 GPa
  • 800°C: 165 GPa
  • 900°C: 153 GPa
  • 1000°C: 143 GPa

High-Temperature Mechanical Properties of alloy C-263 bars:

  • 20°C:
    • Yield strength: 585 MPa
    • Tensile strength: 1004 MPa
    • Elongation: 45 %
    • Reduction of area: 41 %
  • 100°C:
    • Yield strength: 550 MPa
    • Tensile strength: 958 MPa
    • Elongation: 44 %
    • Reduction of area: 44 %
  • 200°C:
    • Yield strength: 520 MPa
    • Tensile strength: 911 MPa
    • Elongation: 44 %
    • Reduction of area: 47 %
  • 300°C:
    • Yield strength: 505 MPa
    • Tensile strength: 880 MPa
    • Elongation: 45 %
    • Reduction of area: 50 %
  • 400°C:
    • Yield strength: 490 MPa
    • Tensile strength: 849 MPa
    • Elongation: 46 %
    • Reduction of area: 51 %
  • 500°C:
    • Yield strength: 500 MPa
    • Tensile strength: 834 MPa
    • Elongation: 46 %
    • Reduction of area: 52 %
  • 600°C:
    • Yield strength: 490 MPa
    • Tensile strength: 819 MPa
    • Elongation: 43 %
    • Reduction of area: 50 %
  • 700°C:
    • Yield strength: 495 MPa
    • Tensile strength: 772 MPa
    • Elongation: 27 %
    • Reduction of area: 34 %
  • 800°C:
    • Yield strength: 460 MPa
    • Tensile strength: 587 MPa
    • Elongation: 15 %
    • Reduction of area: 26 %
  • 900°C:
    • Yield strength: 145 MPa
    • Tensile strength: 232 MPa
    • Elongation: 34 %
    • Reduction of area: 58 %
  • 1000°C:
    • Yield strength: 70 MPa
    • Tensile strength: 108 MPa
    • Elongation: 69 %
    • Reduction of area: 72 %

High-Temperature Mechanical Properties of alloy C-263 sheets:

  • 20°C:
    • Yield strength: 580 MPa
    • Tensile strength: 973 MPa
    • Elongation: 39 %
  • 100°C:
    • Yield strength: 515 MPa
    • Tensile strength: 896 MPa
    • Elongation: 40 %
  • 200°C:
    • Yield strength: 500 MPa
    • Tensile strength: 849 MPa
    • Elongation: 41 %
  • 300°C:
    • Yield strength: 475 MPa
    • Tensile strength: 834 MPa
    • Elongation: 42 %
  • 400°C:
    • Yield strength: 470 MPa
    • Tensile strength: 816 MPa
    • Elongation: 43 %
  • 500°C:
    • Yield strength: 490 MPa
    • Tensile strength: 803 MPa
    • Elongation: 43 %
  • 600°C:
    • Yield strength: 490 MPa
    • Tensile strength: 788 MPa
    • Elongation: 41 %
  • 700°C:
    • Yield strength: 475 MPa
    • Tensile strength: 757 MPa
    • Elongation: 23 %
  • 800°C:
    • Yield strength: 440 MPa
    • Tensile strength: 556 MPa
    • Elongation: 20 %
  • 900°C:
    • Yield strength: 135 MPa
    • Tensile strength: 201 MPa
    • Elongation: 49 %
  • 1000°C:
    • Yield strength: 70 MPa
    • Tensile strength: 108 MPa
    • Elongation: 65 %

Stress Rupture requirements:

  • 650°C, 100h: 531 MPa
  • 650°C, 1000h: 441 MPa
  • 705°C, 100h: 414 MPa
  • 705°C, 1000h: 310 MPa
  • 760°C, 100h: 290 MPa
  • 760°C, 1000h: 193 MPa
  • 815°C, 100h: 172 MPa
  • 815°C, 1000h: 103 MPa
  • 870°C, 100h: 97 MPa
  • 870°C, 1000h: 51 MPa
  • 930°C, 100h: 50 MPa
  • 930°C, 1000h: 28 MPa

Creep Resistance - stress to produce 1% creep:

  • 650°C, 100h: 517 MPa
  • 650°C, 1000h: 400 MPa
  • 705°C, 100h: 372 MPa
  • 705°C, 1000h: 283 MPa
  • 760°C, 100h: 255 MPa
  • 760°C, 1000h: 172 MPa
  • 815°C, 100h: 152 MPa
  • 815°C, 1000h: 83 MPa
  • 870°C, 100h: 76 MPa
  • 870°C, 1000h: 41 MPa
  • 930°C, 100h: 39 MPa
  • 930°C, 1000h: 21 MPa

Thermal Stability - Ultimate tensile strength in a given temperature after staying in the temperature for the given time:

  • 760°C, 0h: 689 MPa
  • 760°C, 8000h: 577 MPa
  • 815°C, 0h: 537 MPa
  • 815°C, 8000h: 404 MPa
  • 870°C, 0h: 341 MPa
  • 870°C, 8000h: 176 MPa

Corrosion Resistance

Heat Resistance / High-Temperature Oxidation - good resistance up to 1000°C.

1008h long static oxidation test results (6 cycles per 168 h in flowing air):

  • 870°C:
    • Metal loss: 3 μm
    • Average metal affected: 10 μm
  • 925°C:
    • Metal loss: 5 μm
    • Average metal affected: 18 μm
  • 980°C:
    • Metal loss: 23 μm
    • Average metal affected: 127 μm

The results of dynamic oxidation tests in the combustion gas (50 parts of air to 1 part of fuel) flowing at 0.3 mach. At the end of each 30 minutes cycle, samples were air cooled down to 260°C. In total, the samples spent 1000h in the combustion gas:

  • 870°C:
    • Metal loss: 36 μm
    • Average metal affected: 102 μm
  • 980°C:
    • Metal loss: 318 μm
    • Average metal affected: 409 μm

Weldability

Alloy 263 has improved weldability over alloy 80A. It can we welded with any common method. It is not susceptible to post-weld heat treatment cracking and heat-affected-zone cracking. The sources differ as to the pre-weld and post-weld heat treatment:

Haynes® 263 alloy datasheet says a post-weld heat treatment is required, and should consist of a solution anneal followed by an aging treatment.

Nimonic® alloy 263 datasheet states "a pre-weld heat treatment is not neccessary on age-hardened assemblies, but a subsequent age-hardening treatment is desirable after all salvage welding is completed. Materials will age in service if temperatures are above 750°C."

VDM Alloy C-263 datasheet says the material should be in the annealed condition before welding, and recommends diffusion annealing after welding.

Welding products: S NI 7263 / NiCo20Cr20MoTi, BS 2901 NA38, 2.4650

Heat Treatment, Working and Machining

Recommended work and heat treatment parameters:

  • Hot working: 1170-950°C; water quench
  • Solution-treatment: 1140-1160°C; rapid air cool / water quench
  • Age-hardening: 785-815°C; 8h; air cool
  • Intermediate annealing: 1070-1090°C; 4-6 min; air cool
  • Homogenizing (treatment): 1150°C; 1h; air cool

During the final hot working operation, the temperature must not exceed 1120°C. The piece should be water-quenched.

We deliver this steel alloy as:

  • Plates, strips and sheets according to AMS 5872, BS HR 206, AECMA PrEn 2203,2418, DIN 17750
  • Bars, rods and forgings according to AMS 5886, BS HR 10, AECMA PrEn 2199,2201,2200, DIN 17752, DIN 17754
  • Wires according to DIN 17753
  • Pipes according to BS HR 404, DIN 17751, AECMA PrEn 2202

Substitutes, equivalents and other species designations

AMS 5886
AMS 5966
Altemp 263
Nimonic® alloy 263
Nickelvac C-263
Udimet Ni90
Unitemp C-263
VDM Alloy C-263
Nicrofer 5120 CoTi
Haynes® 263
Alloy 263
Alloy C-263
N07263
2.4650
NiCr20Co18Ti
BS HR 10
HR HR 206
BS HR 404
NW7263
NiCo20Cr20Mo5Ti2Al

Need help? Contact us!

Call or send a message, and our representative
will contact you within 24 hours!

We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie preferences
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.