61CrSiV5, 1.2243 - tool steel
61CrSiV5, 1.2243 - Tool steel for cold working according to DIN 17350.
| Standard | Steel Grade | ||||||
|---|---|---|---|---|---|---|---|
| Chemical composition % | |||||||
| C: | Mn: | Si: | P: | S: | Cr: | V: | |
| DIN | 61CrSiV5 - 1.2243 | ||||||
| 0.57 - 0.65 | 0.6 - 0.9 | 0.7 - 1.0 | <0.035 | <0.035 | 1.0 - 1.3 | 0.07 - 0.12 | |
61CrSiV5, 1.2243 - specification and application
Tool steel with increased carbon content reaching hardness of 60 HRC, characterized by high resistance to abrasion, fatigue and good impact strength. The material used in the manufacture of metal shears, blades, cutting tools, dies, punches, drills, cutters, wrenches and caps in basic cold working mechanics.
Mechanical properties:
- Softened state <220 HB
- Heat treated condition 40-62 HRC
- Hardness after tempering at temperature:
- 100C = 62 HRC
- 200C = 60 HRC
- 300C = 57 HRC
- 400C = 52 HRC
- 500C = 48 HRC
- 600C = 40 HRC
Heat treatment:
- Softening at a temperature of 700-740C with cooling in furnace
- Relief annealing at a temperature of 650-680C with cooling in furnace
- Hardening at a temperature of 850-880C with cooling in oil
In the above mentioned grades the company delivers:
Substitutes, equivalents and other species designations
61CrSiV5
61 CrSiV 5
2243
K507
1.2243
AJ30H
61SiCrV5
Need help? Contact us!