60S2, 60S2A, 65Si7, 1.5028, 60Si7, 1.5027 - spring steel

60S2, 60S2A, 65Si7, 1.5028, 60Si7, 1.5027 - spring steel according to PN H-84032, GOST 14959-79

Standard Grade
Chemical composition %
C: Si; Mn: P: S: Cr: Ni: Cu
PN 60S2
0,57-0,65 1,5-1,8 0,6-0,9 <0,04 <0,04 <0,03 <0,04 <0,25
PN 60S2A
0,57-0,63 1,6-2,0 0,6-0,9 <0,03 <0,03 <0,03 <0,40 <0,25
DIN 65Si7 / 1.5028
0,6-0,7 1,5-1,8 0,7-1,0 <0,035 <0,035 - - -
EN 60Si7 / 1.5027
0,57-0,64 1,5-2,0 0,6-0,9 <0,04 <0,04 - - -
NF 61SC7
0,57-0,64 1,6-2,0 0,6-0,9 <0,035 <0,035 - - -
UNI 60Si7
0,57-0,64 1,5-2,0 0,6-0,9 <0,035 <0,035 - - -
AISI 9260
0,55-0,65 1,7-2,2 0,65-1,10 <0,035 <0,040 - - -
GOST 60S2
0,57-0,65 1,5-2,0 0,6-0,9 <0,035 <0,035 <0,03 <0,25 <0,2
JIS SUP6
0,56-0,64 1,5-1,8 0,7-1,0 <0,03 <0,03 - - <0,3
GB/T 60Si2Mn
0,56-0,64 1,5-2,0 0,7-1,0 <0,035 <0,035 <0,35 <0,35 <0,25
GB/T 60Si2MnA
0,56-0,64 1,6-2,0 0,6-0,9 <0,03 <0,03 <0,35 <0,35 <0,25

60S2, 60S2A, 65Si7, 1.5028, 60Si7, 1.5027 – description

Spring steel for hardening in oil with low hardenability, sensitive to decarburisation, insensitive to tempering brittleness.

The steel is used for springing parts, like springs and springs for trams, narrow-gauge railways, motor and transport vehicles subjected to medium loads, flat springs, spiral springs, car springs over 8mm thick, disc springs, torsional shafts. It is recommended that the thickness of a rod made from the steel does not exceed 20mm.

Steel 60S2A is characterized by better strength properties than 60S2.

60S2 - Mechanical and Physical Properties

Physical properties in ambient temperature:

  • Density: 7,68 g/cm3
  • Specific heat capacity: 0,46 kJ/(kg*K)
  • Linear expansion coefficient: 11,0 K-1
  • Thermal conductivity: 18,84 W/(m*K)
  • Electrical resistivity: 0,360 Ω*cm
  • Young's modulus E: 21,0 kG/mm2
  • Shear modulus G: 8,0 kG/mm2

Mechanical properties of 60S2 steel:

  • Bars:
    • Diameter cone impression: > 3,5 mm
    • Hardness annealed: 269 HB
    • Hardness raw cond.: 302 HB
    • Percent reduction of area Z: > 25 %
    • Elongation A: > 6 %
    • Tensile strength Rm: > 1270 MPa
    • Yield strength Re: > 1175 MPa
  • Screw cylindrical springs:
    • Generally:
      • Hardness: 41,5-48,5 HRC
      • Hardness: 375-444 HB
    • Cushioning units:
      • Hardness: 41,5-50,5 HRC
  • Helical springs:
    • Generally:
      • Hardness: 40,0-46,5 HRC
      • Hardness: 375-444 HB
    • Spring hardening:
      • Hardness: 42-49 HRC

Mechanical properties of 60S2A steel:

  • Bars:
    • Hot-rolled or hot-forget and drawn:
      • Yield strength Re: > 1375 MPa
      • Tensile strength Rm: > 1570 MPa
      • Elongation A: > 6 %
      • Percent reduction of area Z: > 20 %
      • Hardness - raw cond.: 302 HB
      • Hardness - annealed cond.: 269 HB
      • Diameter cone impression: > 3,5 mm
  • Screw cylindrical springs:
    • Generally:
      • Hardness: 41,5-48,5 HRC
      • Hardness: 375-444 HB
    • Cushioning units:
      • Hardness: 41,5-50,5 HRC
  • Helical springs:
    • Generally:
      • Hardness: 40,0-46,5 HRC
      • Hardness: 375-444 HB
    • Spring hardening:
      • Hardness: 42-49 HRC
  • A clamp of spring rod for mounting rails:
    • Hardness: 42,0-50,5 HRC
  • Spring coldrolled strip:
    • Cold-rolled - Thickness: 0,1-4,0 mm - Tensile strength Rm: 780-1180 MPa
    • Annealed - Thickness: 0,1-4,0 mm
      • Elongation A: > 8 %
      • Tensile strength Rm: < 880 MPa

Heat treatment and working

Recommended working and heat treatment parameters for 60S2 alloy:

  • Forging: 1180-800 °C
  • Rolling: 1180-850 °C
  • Quenching: 860-880 °C / o,w
  • Tempering: 440-480 °C
  • Normalizing annealing: 840-860 °C
  • Soft annealing: 640-680 °C

Recommended cooling methods for plastic forming:

Hot rolling, where the charge is a raw ingot, cold or hot, depending on the thickness of the rolled product:

  • up to 50mm - free cooling in air.
  • 51-150mm - free cooling in a stack or in a pit - open, or covered and unheated with a thermostat set on 100°C.
  • 151-200mm - cooling in a covered and unheated pit with a thermostat set on to 100°C.
  • above 200mm - dehydrogenation

Hot rolling, where the charge is cold billet or slab, rolled or forged, depending on the thickness of the rolled product:

  • up to 100mm - free cooling in air.
  • 101-150mm - free cooling in a stack or in a pit - open, or covered and unheated with a thermostat set on 100°C.
  • 151-200mm - cooling in a covered and unheated pit with a  thermostat set on to 100°C.

Hot forging, where the charge is a raw ingot, cold or hot, depending on the forged product thickness:

  • up to 50mm - free cooling in air.
  • 51-200mm - cooling in insulating material or in the unheated, covered pit, in both cases up to approx. 100°C.
  • over 200mm - anti-flash annealing

Hot forging, where the charge is cold-rolled billet or slab, depending on the thickness of the forged product:

  • up to 100mm - free cooling in air.
  • 101-300mm - cooling in insulating material or in the unheated, covered pit, in both cases up to approx. 100°C.
  • over 300mm - cooling with the furnace or in the covered pit, heated to 100°C.

We deliver this steel alloy as:

Substitutes, equivalents and other species designations

60S2
60S2-Sh
60S2-VD
60S2G
60Si2Mn
60Si2MnA
60Si7
61SC7
65S7
71S7
65Si7
71Si7
60Si7
SUP6
SUP7
60S2A
SPS3
SPS4
9260
H92600
C2332

Need help? Contact us!

Call or send a message, and our representative
will contact you within 24 hours!

We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie preferences
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.