45HNMF, 45ChNMFA, 45ChN2MFA - alloy steel

45HNMFA, 45HN2MFA alloy structural steel for the most high performance engine parts and engines according to PN-72/H-84030 and PN-89/H-84030/04.

Standards Steel Grades
Chemical Composition %
C: Mn: Si: P: S: Cr: Mo: Ni: V: Ti: Cu: N: W:
PN 45HNMF
0.42 - 0.50 0.5 - 0.8 0.17 - 0.37 <0.035 <0.035 0.8 - 1.1 0.2 - 0.3 1.30 - 1.8 0.10 - 0.20 - <0.30 - -
PN 45HNMFA
0.42 - 0.50 0.5 - 0.8 0.17 - 0.37 <0.025 <0.025 0.8 - 1.1 0.2 - 0.3 1.30 - 1.8 0.10 - 0.20 - <0.30 - -
GOST 45ChN2MFA - 45KhN2MFA - 45ХН2МФА
0.42 - 0.50 0.5 - 0.8 0.17 - 0.37 <0.025 <0.025 0.8 - 1.1 0.2 - 0.3 1.30 - 1.8 0.10 - 0.18 <0.03 <0.30 <0.008 <0.2
GOST 45ChNMFA - 45KhNMFA - 45ХНМФА
0.42 - 0.50 0.5 - 0.8 0.17 - 0.37 <0.025 <0.025 0.8 - 1.1 0.2 - 0.3 1.30 - 1.8 0.10 - 0.18 <0.03 <0.30 <0.008 <0.2
PN L45HN2MF
0.40 - 0.50 0.5 - 0.8 0.30 - 0.60 <0.035 <0.035 1.2 - 1.4 0.4 - 0.6 1.60 - 2.0 0.15 - 0.25 - - - -

Structural steel 45HNMFA/45HN2MFA - description and specification

45HNMF steel has a very high hardening capacity, toughness, torsion, abrasion and wear resistance, which achieves the best mechanical properties after hardening in the oil with a dimensions of 170mm.

Products of this grade are designed for heavy-duty parts of engines, motor vehicles and even parts of mining machines. Despite their high quality, the products of this grade are practically non-weldable.

Materials of the 45HNMF grade are used, among others, for parts of mining machinery, parts of rock drills, heavy-duty parts of aircrafts such as chassis, crankshafts, gearbox shafts, and connecting rods.

General mechanical properties of 45HNMFA/45HN2MFA steel

Mechanical properties of 45HNMF
Tensile strengthRm> 1470 MPa
Yield pointRe> 1325 MPa
ElongationA> 7 %
ContractionZ>35 %
Notch toughnessKCU> 40 J
Densityρ7.86 kg/dm3
HardnessHB< 269 HB

45HNMFA / 45HN2MFA mechanical properties for individual dimensions

PropertiesDimensions
<16mm16 - 40mm40 - 100mm100 - 160mm160 - 250mm
Yield pointRe1320 - 1520 MPa1080 - 1270 MPa930 - 1080 MPa740 - 880 MPa740 - 880 MPa
Tensile strengthRm1470 - 1670 MPa1270 - 1470 MPa1080 - 1270 MPa880 - 1080 MPa880 - 1080 MPa
Notch toughnessKCU40 - 80 J50 - 100 J50 - 100 J40 - 80 J40 - 80 J

Heat treatment of 45HNMFA / 45HN2MFA steel

ProcessCooling typeTemperatures
Normalizing annealingslow680 - 720℃
Softening annealingin air850 - 880℃
Hardeningin oil830 - 860℃
Temperingin air500 - 620℃

In the 45HNMFA grade the company supplies:

Substitutes, equivalents and other species designations

45ChN2MFA
45KhN2MFA
45ХН2МФА
45ChNMFA
45KhNMFA
45ХНМФА
K24070
K 24070
45CrNiMoVA
UNS K24045
UNS K 24045
ASTM A290
L45HN2MF
UNS K24245
UNS K 2425
ASTM A291

Need help? Contact us!

Call or send a message, and our representative
will contact you within 24 hours!

We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie preferences
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.