37HS, 38ChS, 38KhS - alloy structural steel

37HS - Chromium-silicon alloy structural steel for construction of heavy-duty and load-bearing parts for thermal improvement in accordance with PN-72 / H-84030.

StandardSteel Grades
Chemical Composition %
C:Mn:Si:P:S:Cr:Mo:Ni:V:Ti:Cu:W:N:
PN37HS
0.34 - 0.420.3 - 0.61.0 - 1.4<0.035<0.0351.3 - 1.6-<0.3-----
GOST38HS - 38ChS - 38KhS - 38ХС
0.34 - 0.420.3 - 0.61.0 - 1.4<0.035<0.0351.3 - 1.6<0.15<0.3<0.05<0.03<0.30<0.2<0.008
БДС38ChS
0.34 - 0.420.3 - 0.61.0 - 1.4<0.035<0.0351.3 - 1.6<0.15<0.3<0.05<0.03<0.30<0.2-
ČSN
STN
ČSN 14 341 - ČSN 14341
0.34 - 0.420.3 - 0.61.0 - 1.3<0.035<0.0351.3 - 1.6-------
GOST38ChS-Sh - 38KhS-Sh - 38ХС-ш
0.34 - 0.420.3 - 0.61.0 - 1.4<0.025<0.0151.3 - 1.6<0.15<0.3<0.05<0.03<0.25<0.2<0.008
GB/T38CrSi - A21382 - A 21382
0.35 - 0.430.3 - 0.61.0 - 1.3<0.035<0.0351.3 - 1.6<0.15<0.3--<0.30--

Steel 37HS - specification and application

Enhanced hardening steel for heat improvement demonstrating its properties after hardening in oil and tempering. It is abrasion-resistant, suitable for large and variable loads. For heavy-duty, high wear and torsion resistant parts, medium-sized heavy duty machines such as friction discs, cams, clutch discs, gears, camshafts, studs, axles, screws and even suction valves

Also used in medium-sized cars, excavators or tractors. 37HS steel is difficult to weld.

37HS also features spring steel properties with low tempering - high strength, wear resistance, elasticity and plasticity.

Mechanical and physical properties

  • Tensile strength Rm ≥ 930 MPa
  • Yield point KU2 ≥ 56 J
  • Elongation A ≥ 12%
  • Contraction Z ≥ 50%
  • Density ρ = 7.74 - 7.85 kg/dm3
  • Electrical resistance at 20℃, ρ = 0.20 ⋅ 10-4 Ω ⋅ cm
  • Specific heat (capacity) at 20℃, cp = 0.11 cal/(g ⋅ ℃)
  • Hardness in a softened state, HB = max. 255
  • Hardness after drawing in the softened state, HB = max. 255
  • Hardness after drawing in the hardened state, HB = max. 293
PropertyDimensions and values
16 - 40mm40 - 100mm100 - 160mm160 - 250mm
Tensile strengthRm≥ 930 MPa≥ 830 MPa≥ 740 MPa≥ 740 MPa
Notch toughnessKU2≥ 30 J≥ 30 J≥ 30 J≥ 30 J
Yield pointRe≥ 740 MPa≥ 640 MPa≥ 540 MPa≥ 540 MPa
ContractionZ≥ 50%≥ 55%≥ 60%≥ 60%
ElongationA≥ 12%≥ 14%≥ 15%≥ 15%

Thermal treatment

Heat treatment - process and temperatures
Normalizing annealingcooling in calm air900 - 930℃
Softening annealingslow cooling680 - 720℃
Hardeningin oil880 - 990℃
Odpuszczaniein oil or water530 - 670℃
Tempering for elastic properties250 - 280℃

Longitudinal modulus of elasticityE

Longitudinal modulus of elasticityE ⋅ 10-3
20℃ 100℃ 200℃ 300℃ 400℃
21.0 kG/mm2 19.5 kG/mm2 18.5 kG/mm2 - 17.5 kG/mm2

Welding, joining and cutting of 37HS steel

Semi-finished products mode of 37HS grade steel before cutting should be preheated to 250 - 300℃. The steel can be cut with propane-butane-oxygen torch, oxyacetylene blowpipe, or plasma torch. After the treatment the product should be cooled in calm air.

37HS can also be joined in an softened annealed condition or heat treated - resistance welding, friction welding or electric welding. However, be sure to select the optimum parameters in narrower ranges than the parameters for low carbon steels.

37HS is not easy to weld, therefore welding should be avoided and should be used in exceptional cases in a softened state. As with cutting, steel should be heated to a suitable temperature depending on the dimensions of the product. 37HS steel is arc-welded with electrodes - ES1.76, ES1.55, ES1.50, ES18-8-6 or CO2 welding - SP1GS.

Steel is recommended to be welded in a softened state. In the case of welding of heat-treated parts, the area around the jointing sites will have worse endurance properties than in the welded locations, so it should be welded immediately before the material has cooled below the heating temperature, the material at the joints is to be heat-treated or annealed.

In the absence of heat treatment, the steel should be cooled with asbestos-based mats, cooled in hot sand when removed from the furnace, or slowly cool the furnace together with the steel. Prior to welding large products or larger sections, it is recommended to carry out interoperative relaxing annealing.

37HS heating temperatures before welding
dimensionstemperature
≤ 15mm150 - 250℃
15 - 25mm200 - 300℃
≥ 25mm250 - 350℃

Substitutes, equivalents and other species designations

38HS
38ChS
38KhS
38ХС
ČSN 14 341
ČSN 14341
38ChS-Sh
38KhS-Sh
38ХС-ш
38CrSi
A21382
A 21382

Need help? Contact us!

Call or send a message, and our representative
will contact you within 24 hours!

We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie preferences
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.