30CrNiMo8, 1.6580 - engineering steel

30CrNiMo8, 1.6580, 30NCD8 - alloyed structural steel for heat treatment according to EN 10083-3, EN 10269.

Standard Steel Grade
Chemical composition %
C: Mn: Si: P: S: Cr: Ni: Mo: Cu:
EN 30CrNiMo8 - 1.6580
0.26 - 0.34 0.3 - 0.6 <0.4 <0.025 <0.035 1.8 - 2.2 1.8 - 2.2 0.3 - 0.5 -
PN 30H2N2M
0.26 - 0.34 0.3 - 0.6 0.17 - 0.37 <0.035 <0.035 1.8 - 2.1 1.8 - 2.1 0.25 - 0.35 <0.2
NF 30CND8 / 30NCD8
0.26 - 0.33 0.3 - 0.6 0.1 - 0.4 <0.030 <0.025 1.8 - 2.2 1.8 - 2.2 0.3 - 0.5 -
ISO 31CrNiMo8
0.27 - 0.34 0.3 - 0.6 0.1 - 0.4 <0.035 <0.035 1.8 - 2.2 1.8 - 2.2 0.3 - 0.5 -

30CrNiMo8, 1.6580 - specification and application

Alloyed structural steel with medium hardenability designed for heavy duty components, characterized by high elasticity and strength properties reaching over 1560 N/mm2 at small diameters. When softened, the hardness reaches max. 248 HRB. It is also characterized by its resistance to variable loads and impacts. The material is not suitable for welding and ultimately requires additional preheating. Grade 30CrNiMo8 is used for production of heavily loaded parts, shafts and drive axes, steering shafts, crankshafts of engines, screws and elements exposed to temperatures in the power industry.

Mechanical properties of 30CrNiMo8, 1.6580

  • Dimensions <16mm
    • Tensile strength, Rm 1250 - 1450 N/mm2
    • Yield strength, Re: >1050 N/mm2
    • Elongation, A: >9%
    • Necking, Z: >40%
  • Dimensions 16-40mm
    • Tensile strength, Rm 1250 - 1450 N/mm2
    • Yield strength, Re: >1050 N/mm2
    • Elongation, A: >9%
    • Necking, Z: >40%
  • Dimensions 40-100mm
    • Tensile strength, Rm 1100 - 1300 N/mm2
    • Yield strength, Re: >900 N/mm2
    • Elongation, A: >10%
    • Necking, Z: >45%
    • Impact strength, KV: >35 J
  • Dimensions 100-160mm
    • Tensile strength, Rm 1000 - 1200 N/mm2
    • Yield strength, Re: >800 N/mm2
    • Elongation, A: >11%
    • Necking, Z: >50%
    • Impact strength, KV: >45J
  • Dimensions 160-330mm:
    • Tensile strength, Rm >850 N/mm2
    • Yield strength, Re: >630 N/mm2
    • Elongation, A: >12%
    • Impact strength, KV: >45 J
  • Dimensions >330mm
    • Tensile strength, Rm >800 N/mm2
    • Yield strength, Re: >590 N/mm2
    • Elongation, A: >12%
    • Impact strength, KV: >40 J

Heat treatment of 30CrNiMo8, 1.6580 steel

  • Softening annealing at a temperature of 640 - 680℃
  • Normalizing annealing at a temperature of 840 - 860℃
  • Hardening with cooling in oil at 815 - 845℃
  • Tempering with cooling in air at 550 - 650℃

Substitutes, equivalents and other species designations

30ChN2MA
30HN2MA
30ХН2МА
30NCD8
30CND8
31CrNiMo8
NCMo6 Z
31CrNiMo8H
31CrNiMo8HH
31CrNiMo8HL
SNCM431
30MoCrNi20
C5432

Need help? Contact us!

Call or send a message, and our representative
will contact you within 24 hours!

We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie preferences
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.