18HGT, 18ChGT, 21TiMnCr12 - case-hardening steel

18HGT, 18ChGT, 21TiMnCr12, CSN 14223 – case-hardening steel according to PN H-84030/02, GOST 4543-71.

Standard Grade
Chemical composition %
C: Si: Mn: P: S: Cr: Ni: Ti:
PN 18HGT
0.17-0.23 0.17-0.37 0.8-1.1 <0.035 <0.035 1.0-1.3 <0.3 0.05-0.12
GOST 18ChGT
0.17-0.23 0.17-0.37 0.8-1.1 <0.035 <0.035 1.0-1.3 <0.3 0.03-0.09
GOST 18ChGT-Sh
0.17-0.23 0.17-0.37 0.8-1.1 <0.025 <0.015 1.0-1.3 <0.3 0.03-0.09
ČSN 14223
0.17-0.23 0.17-0.37 0.8-1.1 <0.035 <0.035 1.0-1.3 - 0.04-0.10
STAS 21TiMnCr12
0.17-0.23 0.17-0.37 0.8-1.1 <0.035 <0.035 1.0-1.3 <0.3 0.03-0.09

18HGT, 18ChGT, 21TiMnCr12, 14223 – description

Steel used for heavily loaded structural parts with high core strength required, such as gears and gearbox shafts. It has a high resistance to overheating and does carburize quickly at high temperature. Weldable, machinable and cuttable steel. Weld before and after carburizing.

Physical and mechanical properties

Here You can find the mechanical properties of selected alloys. Despite their similarities, they clearly differ.

Mechanical properties Standard / Grade
PN GOST ČSN STAS
18HGT 18ChGT 14223 21TiMnCr12
Yeld strenght: Rm > 830 MPa > 885 MPa > 740 MPa > 880 MPa
Tensile strenght: Rm > 980 MPa > 980 MPa 880-1180 MPa 1180-150 MPa
Elongation: A5 9 % 9 % 10 % 9 %
Impact KCU, 20°C: KCU2 J/cm2 80 J/cm2 79 J/cm2 69 J/cm2 -
Hardness in annealed cond. HB 217 HB 217 HB 197 HB 217 HB

Mechanical properties after hardening:

  • Diameter D: 11 mm
    • Tensile strength Rm: 920-1270 MPa
    • Yield strength Re: min 600 MPa
    • Elongation A: min 9 %
    • Impact Value KU: min 25 J
  • Diameter D: 30 mm
    • Tensile strength Rm: 820-1170 MPa
    • Yield strength Re: min 540 MPa
    • Elongation A: min 10 %
    • Impact Value KU: min 25 J
  • Diameter D: 63 mm
    • Tensile strength Rm: 710-1060 MPa
    • Yield strength Re: min 480 MPa
    • Elongation A: min 11 %
    • Impact Value KU: min 25 J

Heat treatment and plastic working

Following parameters are recommended for working and heat treatment

Treatment Grade
PN GOST ČSN STAS
18HGT 18ChGT 14223 21TiMnCr12
Quenching Temperature 810-830℃ 880-950℃ 850-880℃ 875-910℃
Cooling oil air oil oil
Tempering Temperature 200℃ 200℃ 150-200℃ 170-190℃
Cooling air, oil furnance, oil air, oil air, oil

Temperatures of other technological processes of heat and thermo-chemical treatment:

  • Carbonitriding: 860-930℃
  • Hardening and carburizing: 850-880℃. Cooling in water or oil.
  • Annealing after carburizing: 660-680℃
  • Hardening II after carburizing: 810-830℃. Cooling in water or oil.
  • Carburizing tempering: 150-200℃.

We deliver this steel alloy as:

  • Bars, strips and reels
  • Rods

Substitutes, equivalents and other species designations

18HGT
6-K1
18ChGT
14223
18CrMnTi5
21TiMnCr12
20MC5
18ChGT-Sh
18ChGTA
18ChGTA-VD
20CrMnTi
20TiMnCr12

Need help? Contact us!

Call or send a message, and our representative
will contact you within 24 hours!

We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie preferences
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.