115CrV3, 1.2210 - tool steel
Tool steel for cold working 115CrV3, 1.2210, 11HF - "Silver steel" according to DIN 17350.
| Standard | Steel Grade | |||||||||
|---|---|---|---|---|---|---|---|---|---|---|
| Chemical composition % | ||||||||||
| C: | Mn: | Si: | P: | S: | Cr: | Ni: | V: | Mo: | W: | |
| DIN | 115CrV3 - 1.2210 | |||||||||
| 1.10 - 1.25 | 0.20 - 0.40 | 0.15 - 0.30 | <0.03 | <0.03 | 0.5 - 0.8 | - | 0.07 - 0.12 | - | - | |
| PN | NW1 | |||||||||
| 1.10 - 1.25 | 0.15 - 0.45 | 0.15 - 0.40 | <0.030 | <0.030 | <0.35 | - | <0.15 | <0.20 | 1.10 - 1.50 | |
| GOST | 11ChF - 11ХФ | |||||||||
| 1.05 - 1.15 | 0.40 - 0.70 | 0.10 - 0.40 | <0.030 | <0.030 | 0.4 - 0.7 | <0.4 | 0.15 - 0.30 | - | <0.20 | |
115CrV3, 15CrNi6, 1.2210, NW1 - specification and application
Grade with low hardenability and sensitivity to overheating, low tendency to crack when hardened in water, high abrasion resistance, good cutting properties and durability of the knife. It is also characterized by low resistance to tempering. Material used for the production of cutters, drills, circular saws for metal cutting, reamers, coin and medal punches, tools for cutting wood, paper, tobacco, and rubber. It is also used for the production of dies, threaders, drills, circular knives, jaws for cutting threads and nails, engraving tools, bimetal knives, and countersinks. In the original Bright steel NW1, tungsten at a concentration of 1.10-1.50% was present.
Mechanical properties of 115CrV3, 1.2210
- Hardness after hardening >62 HRC
- Hardness after hardening and tempering at temperature:
- 200C = >62 HRC
- 250C = >62 HRC
- 300C = 60 HRC
- 350C = 57.4 HRC
- 400C = 53.9 HRC
- 450C = 50.3 HRC
- 500C = 46.2 HRC
- 550C = 41.9 HRC
Heat treatment - processes and temperatures:
- Softening annealing at a temperature of 690 - 710C
- Relief annealing at a temperature of 600 - 700C
- Annealing at a temperature of 780 - 800C
- Tempering at a temperature of 200 - 320C
In the above mentioned grades the company delivers: