1.4122, X39CrMo17-1, 1.2316, X38CrMo16 - stainless steel

X39CrMo17-1, 1.4122, X38CrMo16, 1.2316 - Martensitic stainless and tool steel in accordance with ISO 4957, EN 10088-3.

Standard Steel Grade
Chemical composition %
C: Mn: Si: P: S: Cr: Mo: Ni:
EN X39CrMo17-1 - 1.4122
0.33 - 0.45 <1.5 <1.0 <0.04 <0.03 15.5 - 17.5 0.8 - 1.3 <1.0
ISO X38CrMo16 - 1.2316
0.33 - 0.45 <1.5 <1.0 <0.03 <0.03 15.5 - 17.5 0.8 - 1.3 <1.0
DIN X36CrMo17 - 1.2316
0.33 - 0.43 <1.0 <1.0 <0.03 <0.030 15.0 - 17.0 1.0 - 1.3 <1.0
NF Z38CD16-01
0.33 - 0.45 <1.0 <1.0 <0.04 <0.015 15.5 - 17.5 0.8 - 1.3 -
NF Z35CD17
0.33 - 0.45 <1.5 <1.0 <0.03 <0.03 15.5 - 17.5 0.8 - 1.3 <1.0
PN 3H17M
0.33 - 0.43 <1.0 <1.0 <0.045 <0.030 15.5 - 17.5 1.0 - 1.3 <1.0

X39CrMo17-1, 1.4122, X38CrMo16, 1.2316 - specification and application

Chrome-molybdenum stainless martensitic steel for quenching, showing the structure of perlite after heat treatment. After hardening and tempering it reaches the hardness of 220 - 275 HB depending on the dimensions.

It shows corrosion resistance in environments containing nitric acid in low concentrations, nitrate, bicarbonate and ammonium nitrite, zinc carbonate, manganese chloride, vinegar, potassium nitrate and mixtures, sodium chloride, sodium hydroxide, water, steam, acetone, alcohol, gasoline, glycerine, chloroform, oleic acid and salicylic acid.

It is not resistant to chlorine solutions, hydrochloric acid, acetic acid, hydrofluoric acid, orthophosphoric acid, potassium sulphate, sulphuric acid, citric acid, lactic acid, formic acid, oxalic acid and tartaric acid.

The conclusion from the chemical composition cannot be ignored without stating that grade 1.4122 and derivatives are more suitable in the form of a product for the production of mechanical elements that exhibit basic corrosion resistance than vice versa. The product has excellent mechanical properties in basic corrosive environments, if properly treated, does not corrode, exhibits good properties at elevated temperatures, good polishing properties, is unfortunately not suitable for welding and is not resistant to intergranular corrosion.

The closest equivalent of 1.4122 / X39CrMo17-1 classified as a tool steel is X36CrMo17 / 1.2316. 1.4122 is a great alternative to 4H13 / X46Cr13 / 1.4034 grade - it has similar properties and much better corrosion resistance. It is used in industry for the production of shafts, gears, spindles, bodies and moulds for the production of plastics, metal casting, mandrels, valves, toolholders, screws, pins and surgical instruments.

Mechanical properties X39CrMo17-1, 1.4122 in accordance with EN 10088-3, EN 10088-1:

  • Delivery condition +A
    • Dimensions 63-160mm
      • Tensile strength, Rm <900 MPa
      • Hardness, HB< 280
    • Dimensions 40-63mm
      • Tensile strength, Rm <930 MPa
      • Hardness, HB< 290
    • Dimensions 16-40mm
      • Tensile strength, Rm <980 MPa
      • Hardness, HB< 310
    • Dimensions <16mm
      • Tensile strength, Rm <1000 MPa
      • Hardness, HB< 340
  • Delivery condition +QT750
    • Dimensions <10mm
      • Tensile strength, Rm 800 - 1050 MPa
      • Yield strength, Re >650
      • Elongation, A: >8%
    • Dimensions 10-16mm
      • Tensile strength, Rm 800-1050 MPa
      • Yield strength, Re >600
      • Elongation, A: >8%
    • Dimensions 16-40mm
      • Tensile strength, Rm 750 - 1050 MPa
      • Yield strength, Re >550
      • Elongation, A: >10%
      • Impact strength, KV: >14 J
    • Dimensions >40mm
      • Tensile strength, Rm 750 - 950 MPa
      • Yield strength, Re >550
      • Elongation, A: >12%
      • Impact strength, KV: >10 J
  • Other physical and mechanical properties:
    • Modulus of elasticity E = 215 GPa
    • Thermal conductivity λ = 15 W ⋅ m-1 ⋅ K-1
    • Thermal capacity cp = 430 J ⋅ kg-1 ⋅ K-1
    • Resitivity, Ω: 0.80 mkOhm * m
    • Linear expansion coefficient, α: 10,4 * 10-6 K-1

Operation at elevated temperatures of 1.4122, X39CrMo17-1 in +QT750 condition:

Properties Temperatures
100℃ 150℃ 200℃ 250℃ 300℃ 350℃ 400℃
Yield strength, Rp0,2 (MPa) >540 >535 >530 >520 >510 >490 >470
Modulus of elasticity, E (GPa) 212 - 205 - 200 - 190
Linear expansion coefficient, α (* 10-6 K-1) 10.4 - 10.8 - 11.2 - 11.6

Mechanical properties of 1.2316, X38CrMo16 according to ISO 4957

  • Improved condition +QT - hardness 300 HB

Heat treatment - processes and temperatures:

  • Annealing at a temperature of 750 - 850℃
  • Hardening at 980 - 1060℃
  • Tempering at 650 - 750℃
  • Cooling in oil
  • Plastic forming at 1100 - 800℃

In the above mentioned grades we supply the following metallurgical products:

Substitutes, equivalents and other species designations

35MoCr165
GX35CrMo17
Z38CD16-1
Z35CD17
35Х16НМ
40Х16М
X38CrMo16
420Mod
X36CrMo17
X35CrMo17
35H16NM
40H16M

Need help? Contact us!

Call or send a message, and our representative
will contact you within 24 hours!

We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie preferences
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.