1.2328, 45CrMoV7, 40Ch2GMF - Tool die steel
1.2328, 45CrMoV7, 40Ch2GMF - Tool die steel, data according to DIN 17350
| Standard | Grade | ||||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Chemical composition % | |||||||||||||||
| C: | Si: | Mn: | P: | S: | Cr: | Mo: | V: | ||||||||
| DIN | 1.2328 - 45CrMoV7 | ||||||||||||||
| 0.42-0.47 | 0.2-0.3 | 0.85-1.00 | <0.03 | <0.03 | 1.7-1.9 | 0.25-0.30 | 0.05 | ||||||||
| GOST | 45Ch2GMF - 40Х2ГМФ | ||||||||||||||
| 0.42-0.47 | 0.2-0.3 | 0.85-1.00 | <0.03 | <0.03 | 1.7-1.9 | 0.25-0.30 | 0.05 | ||||||||
1.2328, 45CrMoV7, 40Ch2GMF – description
Tool steel used for cold working die tools, stamps and drifters. It has good wear resistance.
The steel is meant to be air-hardened, which reduces the risk of deformations and cracks during the heat treatment. It has good hardenability but is susceptible to tempering, thus requires proper temperature during work.
Physical and mechanical properties
1.2328 - general physical and mechanical properties in ambient temperature:
- Density: 7.85 g/m3
- Hardness in soft annealed condition: < 250 HB
Heat treatment and working
Recommended working and heat treatment parameters for 1.2328 alloy:
- Forging: 1000-850 °C
- Rolling: 1000-850 °C
- Quenching: 840-860 °C
- Soft annealing: 690-730 °C
We deliver this steel alloy as:
- Forgings
- Rods
- Pipes
Substitutes, equivalents and other species designations
Need help? Contact us!
Call or send a message, and our representative
will contact you within 24 hours!
Write
Call