High-speed tungsten-molybdenum steel HS6-5-2C, S6-5-2, 1.3343, AISI M2 according to ISO 4957, DIN 17350.

 

Standard Steel Grade
Chemical Composition %
C: Mn: Si: P: S: Cr: Mo: Ni: V: W: Co:
PN SW7M
0.82 - 0.92 <0.4 <0.5 <0.03 <0.03 3.5 - 4.5 4.5 - 5.5 <0.4 1.7 - 2.1 6.0 - 7.0 <0.5
ISO HS6-5-2C
0.86 - 0.94 <0.4 <0.45 <0.03 <0.03 3.8 - 4.5 4.7 - 5.2 - 1.7 - 2.1 5.9 - 6.7 -
ISO HS6-5-2 - 1.3339
0.80 - 0.88 <0.4 <0.45 <0.03 <0.03 3.8 - 4.5 4.7 - 5.2 - 1.7 - 2.1 5.9 - 6.7 -
DIN S6-5-2 - 1.3343
0.86 - 0.94 <0.4 <0.45 <0.03 <0.03 3.8 - 4.5 4.7 - 5.2 - 1.7 - 2.0 6.0 - 6.7 -
NF Z85WDCV06-05-04-02
0.80 - 0.87 <0.4 <0.5 <0.03 <0.03 3.5 - 4.5 4.6 - 5.3 - 1.7 - 2.2 5.7 - 6.7 -
ASTM UNS T11302 - AISI M2
0.78 - 0.88 0.15 - 0.40 0.20 - 0.45 <0.03 <0.03 3.75 - 4.50 4.5 - 5.5 - 1.75 - 2.20 5.50 - 6.75 -
GOST R6M5 - Р6М5
0.82 - 0.90 <0.5 <0.5 <0.03 <0.25 3.80 - 4.40 4.8 - 5.3 <0.4 1.7 - 2.1 5.5 - 6.5 <0.5

 

S6-5-2, HS6-5-2, 1.3343 - specification and application

High-speed steel with very good efficiency, ductility, resistance to abrasion and torsion, and impact strength used to work with products with a strength of more than 830 MPa. It is used in the production of drills, blades, knives, spiral drills, thread cutting tools, broaching tools, gear tools, milling cutters, mandrel reamers, end milling cutters, and circular saw segments. SW7M / 1.3343 is prone to decarburization and overheating during heat treatment. After hardening and tempering, it achieves hardness above 63 HRC.


Mechanical properties of SW7M, S6-5-2, HS6-5-2C, 1.3343

  • Hardness in +A delivery condition: <269 HB
  • Hardness in +A+C delivery condition: <319 HB
  • Hardness in +A+CR delivery condition: <339 HB
  • Hardness after hardening and tempering:
    • at 300 ℃ = 61,5 HRC
    • at 350 ℃ = 62 HRC
    • at 400 ℃ = 62 HRC
    • at 450 ℃ = 63 HRC
    • at 500 ℃ = 65 HRC
    • at 550 ℃ = 65 HRC
    • at 600 ℃ = 60 HRC
    • at 650 ℃ = 52 HRC

 


Heat and plastic treatment processes of SW7M, S6-5-2, HS6-5-2C, 1.3343 steel:

  • Softening annealing at a temperature of 800 - 900 ℃
  • Relief annealing at a temperature of 600 - 700℃
  • Heating no. I in a temp. of about 550℃
  • Heating no. II in a temp. of about 850℃
  • Austenitizing at 1190 - 1230 ℃ (hardening in salt bath and oil)
  • Tempering usually in the range of 550 - 570 ℃
  • Forging and rolling at temperatures 1100 - 900 ℃
  • Nitriding in the temperature range of 510 - 530 ℃

 


In the above mentioned grades the company provides:

 


Other replacements and equivalents of the grade:

SW7M, 1.3343, HS6-5-2C, HS6-5-2, S6-5-2, 1.3339, X82WMoCrV6-5-4, X80WMoCrV6-5-4, X 82 WMoCrV 6-5-4, X 80 WMoCrV 6-5-4, R6M5, AISI M2, SKH51, SS 2722, R6, W6Mo5Cr4V2, CSN 19830, 1.3553, SC6-5-2, SC 6-5-2, 1.3341, BS BM2, X82WMo0605KU, X 80 WMo 06 05 KU, RP5, EM2, F-550.A, UNS T11302, AISI M-2, HS 6-5-2 C, S 6-5-2, Р6М5, R6M5.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.