High-speed cobalt-tungsten steel with the addition of Molybdenum HS6-5-2-5, 1.3243, AISI M41 according to ISO 4957, DIN 17350.

 

Standard Steel Grade
Chemical Composition %
C: Mn: Si: P: S: Cr: Mo: Ni: V: W: Co:
PN SK5M
0.85 - 0.95 <0.4 <0.5 <0.03 <0.03 3.5 - 4.5 4.6 - 5.2 <0.4 1.7 - 2.1 6.0 - 6.7 4.5 - 5.5
ISO HS6-5-2-5 - 1.3243
0.87 - 0.95 <0.4 <0.45 <0.03 <0.03 3.8 - 4.5 4.7 - 5.2 - 1.7 - 2.1 5.9 - 6.7 4.5 - 5.0
DIN S6-5-2-5 - 1.3243
0.88 - 0.96 <0.4 <0.45 <0.03 <0.03 3.8 - 4.5 4.7 - 5.2 - 1.7 - 2.0 6.0 - 6.7 4.5 - 5.0
NF Z90WDKCV06-05-05-04-02
0.88 - 0.96 <0.4 <0.5 <0.03 <0.03 3.5 - 4.5 4.6 - 5.3 - 1.7 - 2.2 5.7 - 6.7 4.5 - 5.2
ASTM UNS T11341 - AISI M41
1.05 - 1.15 0.2 - 0.6 0.15 - 0.50 <0.03 <0.03 3.75 - 4.50 3.25 - 4.25 - 1.75 - 2.25 6.25 - 7.00 4.75 - 5.75
GOST R6M5K5 - Р6М5K5
0.84 - 0.92 <0.6 <0.5 <0.03 <0.03 3.8 - 4.5 4.8 - 5.3 <0.4 1.7 - 2.1 5.7 - 6.7 4.7 - 5.2

 

HS6-5-2-5, 1.3243, AISI M41 - specification and application

High-speed steel with very good ductility, high cutting properties and tempering temperature, designed for work with difficult-to-cut materials with high hardness, including austenitic steels.

It is mainly used for special drills and cutters, tools for machining of gears, shape knives, turning and planing knives. SK5M steel is used for machining rims, rollers, wheelsets and cast iron products.


Mechanical properties of HS6-5-2-5, 1.3243, AISI M41 steel

  • Hardness in softening annealed condition +A: 223-285 HB
  • Hardness after hardening and tempering:
    • in a temp. of 300℃ = 62,5 HRC
    • in a temp. of 350℃ = 62 HRC
    • in a temp. of 400℃ = 62 HRC
    • in a temp. of 450℃ = 63 HRC
    • in a temp. of 500℃ = 64 HRC
    • in a temp. of 550℃ = 65 HRC
    • in a temp. of 600℃ = 62,5 HRC
    • in a temp. of 650℃ = 56 HRC
    • in a temp. of 700℃ = 47 HRC

 


Heat and temperatures of processes for HS5 6-5-2-5, 1.3243, AISI M41 steel:

  • Nitriding at temperature of 510 - 530 ℃
  • Softening in the temperature of 800 - 900 ℃
  • Relief annealing at a temperature of 600 - 700℃
  • Heating no. I in a temperature of about 550℃
  • Heating no. II in a temperature of about 850℃
  • Austenitization at 1180 - 1220℃
  • Tempering at temperature of 550 - 570 ℃

 


In the above mentioned grades the company provides:

 


Other indications of grades and substitutes:

SK5M, X85WMoCo6.5.5, X85WMoCo6-5-5, R8, C.9780, SS 2723, HS6-5-2-5, HS 6-5-2-5, S6-5-2-5, S 6-5-2-5, SKH55, AISI M41, M-41, M 41, R6M5K5, SEW 44981, 1.3243, W6Mo5Cr4V2Co5, BM35, UNS T11341, Р6М5K5.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.