Weathering steel / corten steel PN-EN 10025-5

Weathering steels (also known as atmospheric corrosion-resistant steel or Corten steel after trademarked COR-TEN® steel) are structural steels containing small amounts of alloying elements such as copper, phosphorus, silicon, and chromium. These additions significantly improve resistance to atmospheric corrosion while keeping the low cost. Under favorable weather conditions, a relatively stable layer of hydrated iron oxide forms on the steel surface. Unlike ordinary rust, this layer does not flake off or quickly penetrate deeper into the steel. Instead, it develops into an attractive brown “patina”. Weathering steel does not require painting.
Weathering steels can be used for modern architectural elements and structures. Long, dry summers are particularly favorable for the development of the protective layer, while frequent rainfall can accelerate corrosion.

Broadcasting tower in Leeds – a building clad in weathering steel. On the left, its condition in 2005 (Wikimedia, author Mtaylor848). On the right, its condition in 2025 (Google Street Map). Please note different lighting and weather conditions.
COR-TEN® Steel
The COR-TEN® trademark is owned by United States Steel Corporation. According to SSAB, the Swedish-American steelmaker that currently uses the trademark, the chemical composition and properties of these steels are as follows:
SSAB COR-TEN® A steel:
- Chemical composition: C<0.12; Si:0.25-0.75; Mn:0.2-0.5; P:0.07-0.15; S<0.03; Al:0.015-0.06; Cu:0.25-0.55; Cr:0.5-1.25; Ni<0.65
- Yield strength ReH > 310 MPa
- Tensile strength Rm > 450 MPa
- Elongation A > 22%
SSAB COR-TEN® B steel:
- Chemical composition: C<0.19; Si:0.30-0.65; Mn:0.80-1.25; P<0.035; S<0.03; Al:0.020-0.06; V:0.02-0.10; Cu:0.25-0.40; Cr:0.4-0.65; Ni<0.65
- Yield strength ReH > 345 MPa
- Tensile strength Rm > 485 MPa
- Elongation A > 19%
Corten A steel contains phosphorus, which gives it higher corrosion resistance but also makes it more brittle and more difficult to weld. Corten B has typical phosphorus content and an alloying addition of vanadium, which improves its mechanical properties.
Weathering steels according to PN-EN 10025-5
PN-EN 10025-5 specifies the requirements for weathering steels – the standardised equivalents of COR-TEN® steels. The mechanical properties given below apply to products with a thickness of 16 mm. Elongation values are given for longitudinal specimens.
S235J0W / S235J2W steel:
- Chemical composition: C<0.13; Si<0.4; Mn:0.2-0.6; P<0.035; Cr:0.4-0.8; Cu:0.25-0.55; Ni<0.65
- S235J0W: S<0.035; N<0.009
- S235J2W: S<0.030; one of the nitrogen-binding elements: Nb:0.015-0.06; V:0.02-0.012 or Ti:0.02-0.1
- Yield strength ReH > 235 MPa
- Tensile strength Rm > 360 MPa
- Elongation A > 26%
S355J0WP / S355J2WP steel:
- Chemical composition: C<0.12; Si<0.75; Mn<1.0; P:0.06-0.15; Cr:0.3-1.25; Cu:0.25-0.55; Ni<0.65
- S355J0WP: S<0.035; N<0.009
- S355J2WP: S<0.030; one of the nitrogen-binding elements: Nb:0.015-0.06; V:0.02-0.012 or Ti:0.02-0.1
- Yield strength ReH > 355 MPa
- Tensile strength Rm > 470 MPa
- Elongation A > 22%
S355J0W / S355J2W steel:
- Chemical composition: C<0.16; Si<0.50; Mn:0.5-1.5; P<0.35; Cr:0.4-0.8; Cu:0.25-0.55; Ni<0.65
- S355J0W: S<0.035; N<0.009
- S355J2W: S<0.030; one of the nitrogen-binding elements: Nb:0.015-0.06; V:0.02-0.012 or Ti:0.02-0.1
- Yield strength ReH > 355 MPa
- Tensile strength Rm > 470 MPa
- Elongation A > 22%
Composition and alloying elements
Weathering steel achieves improved corrosion resistance at relatively low cost by combining several alloying elements in small amounts. The combined effect of these additions is significantly greater than that of adding a single element in a quantity equal to the total amount of the individual elements.
Phosphorus P in concentrations above 0.1% significantly improves resistance to atmospheric corrosion. However, phosphorus also reduces impact toughness and weldability. This is why it is intentionally present in COR-TEN A® steel, S355J0WP, and S355J2WP, while in other weathering steels it is generally treated as an impurity.
Copper Cu is one of the key alloying elements. Increasing the Cu content from 0.01% to 0.05% reduces the corrosion rate by 2–3 times. However, increasing the copper content above 0.3% has only a minor effect on corrosion resistance. Most weathering steels contain between 0.25 and 0.55% Cu.
Silicon Si at a content of around 0.25% moderately benefits corrosion resistance.
Chromium Cr at a content of around 0.6% significantly improves corrosion resistance without adding excessively to the cost of the steel.
Manganese Mn does not have any effect on corrosion resistance.
Sulfur S reduces corrosion resistance and is therefore considered an impurity.