Hot-Dip and Electrolytic Coatings for Steel Strip

Author:

Piotr Sompoliński

Date added:

Metallic coatings protect steel against corrosion and affect its properties during processing and in service. Learn about the differences between hot-dip galvanization and electrogalvanization, their designations, and how to interpret coating mass and thickness. 

Types and applications

Steel strip can be continuously coated with metals using two main methods: hot-dip coating and electrolytic coating. For economic reasons, hot-dip zinc coatings are the most widely used. The coating forms a physical barrier between the steel and the corrosive environment, with zinc corroding much more slowly than steel because it is more electrochemically active than iron.

Metal-coated strip and sheet are used primarily in the construction and automotive industries. Electrolytically coated strip is also widely used in the manufacture of packaging, household appliances and furniture.

Types of hot-dip coatings:

  • zinc Zn
  • zinc-iron Zn-Fe
  • aluminium Al 
  • zinc-aluminium Zn-Al
  • aluminium-zinc Al-Zn
  • lead-tin Pb-Sn
  • phosphate P

Electrogalvanization types:

  • zinc Zn
  • zinc-nickel Zn-Ni
  • zinc-iron Zn-Fe

Continuously applied hot-dip coatings are produced by immersing steel strip in a bath of molten coating metal, such as zinc or aluminium. Electrogalvanization is done at room temperature.

The table below compares the key characteristics of the different coating types.

Comparison of coating characteristics
Coating Characteristics
Corrosion resistance Deep drawability Weldability
/solderability
Paint adhesion Designation Appearance
Hot-dip Zn good good fair good Z varies
Hot-dip Zn-Fe good very good very good good ZF matt grey
Hot-dip Al excellent
+ highly heat-resistant
poor poor good A attractive
Hot-dip Al-Zn very good
+ heat-resistant
poor poor good AZ attractive
Hot-dip Zn-Al very good good good good ZA varies
Hot-dip Pb-Sn very good very good very good good   unattractive
Hot-dip Phosphate poor     excellent    
Electrogalvanisation Zn good excellent
with a thin coating
fair   ZE  
Electrogalvanisation Zn-Ni very good excellent good   ZN  
Electrogalvanisation Zn-Fe very good good good very good ZnFe  

 

Hot-dip Zn coating process

First, the strip is electrolytically cleaned and then fed into a heat-treatment furnace operating at 730-850°C, where it undergoes recrystallization. The strip is then immersed in a molten zinc bath maintained at 445-465°C. Higher temperatures are undesirable because steel dissolves much more rapidly in zinc above 480°C, which can adversely affect the properties of the coated strip. After leaving the zinc bath, the strip passes through air knives that control the coating thickness. It is then subjected to skin-pass rolling or tension levelling to prevent Lüders lines from forming during cold working and to achieve the required flatness and shape. The final stage is passivation, in which the strip is immersed in or sprayed with a chromic acid solution.

Storing the coated strip in humid conditions can lead to the formation of so-called white rust on the coating surface. This is caused by the formation of zinc carbonate. White rust affects the appearance of the coating, but does not necessarily mean that the coating has been damaged. In fact, the corrosion rate gradually decreases as the corrosion products form. The passivation treatment described above helps protect the coating against white rust.

Rapid cooling after hot-dip coating can supersaturate the ferrite with carbon, reducing ductility and causing strain ageing. To restore ductility, Zn-coated steel may be aged in batch annealing furnaces at temperatures below 300°C. Interstitial-free steel is not susceptible to this loss of ductility.

The same production line can also be used to apply other coatings.

Coating thickness

Coating thickness is one of the most important coating parameters, which is why it is selected according to the customer's requirements. Thin coatings are more readily deformed together with the steel substrate. Very thin coatings, suitable for deep drawing and subsequent painting, can only be produced by electrogalvanizing. Additionally, electrogalvanizing makes it possible to coat only one side of a strip, whereas hot-dip coating always coats both sides.

Coating mass is expressed in g·m⁻². For hot-dip coatings, this value refers to the total coating mass on both sides of the sheet. When electrogalvanizing, the coating mass is specified for one side of the strip.

Hot-dip coated steel grades

Hot-dip coated steel grades intended for cold forming (including drawing) according to PN-EN 10327:

  • DX51D - steel for machine folding and profiling
    • Tensile strength Rm < 500 MPa
    • Elongation A > 22%
  • DX52D - steel for drawing
    • Yield strength Re < 300 MPa
    • Tensile strength Rm < 420 MPa
    • Elongation A > 26%
  • DX53D - steel for deep drawing
    • Yield strength Re < 260 MPa
    • Tensile strength Rm < 380 MPa
    • Elongation A > 30%
  • DX54D - steel for extra-deep drawing
    • Yield strength Re < 220 MPa
    • Tensile strength Rm < 350 MPa
    • Elongation A > 36%
  • DX56D - steel for very deep drawing
    • Yield strength Re < 180 MPa
    • Tensile strength Rm < 350 MPa
    • Elongation A > 39%
  • DX57D - steel for super-deep drawing
    • Yield strength Re < 170 MPa
    • Tensile strength Rm < 350 MPa
    • Elongation A > 41%

Hot-dip coated strip and sheet grades made from structural steel according to PN-EN 10326:

  • S220GD
    • Yield strength Re > 220 MPa
    • Tensile strength Rm > 300 MPa
    • Elongation A > 20%
  • S250GD
    • Yield strength Re > 250 MPa
    • Tensile strength Rm > 330 MPa
    • Elongation A > 19%
  • S280GD
    • Yield strength Re > 280 MPa
    • Tensile strength Rm > 360 MPa
    • Elongation A > 18%
  • S320GD
    • Yield strength Re > 320 MPa
    • Tensile strength Rm > 390 MPa
    • Elongation A > 17%
  • S350GD
    • Yield strength Re > 350 MPa
    • Tensile strength Rm > 420 MPa
    • Elongation A > 16%
  • S550GD
    • Yield strength Re > 550 MPa
    • Tensile strength Rm > 560 MPa

Products and designations

Products are designated by specifying the steel grade, coating type and additional treatment designations, according to the following format: steel + coatingmass-treatment. Examples:

  • DX53D + ZF100-R-B-O - DX53D steel hot-dip coated with a zinc-iron alloy, with a coating mass of 100 g⋅m-2, an R-type finish, improved surface quality (B) and an oiled surface (O).
  • DX53D + ZA130-B-C - DX53D steel hot-dip coated with a zinc-aluminium alloy, with a total coating mass of 130 g⋅m-2 on both sides, improved surface quality (B) and chemical passivation (C).

Steel grades (as listed above, from DX51D to DX57D).

Coating designations:

  • Z - zinc, hot-dip galvanizing
  • ZF - zinc-iron, hot-dip galvanizing
  • AS - aluminium-silicon, hot-dip galvanizing
  • AZ - aluminium-zinc, hot-dip galvanizing
  • ZA - zinc-aluminium, hot-dip galvanizing
  • ZE - zinc, electrogalvanizing
  • ZN - zinc-nickel, electrogalvanizing
  • ZnFe - zinc-iron, electrogalvanizing

Surface treatment designations:

  • C - chemical passivation,
  • O - oiling,
  • CO - chemical passivation followed by oiling,
  • S - with an applied organic coating,
  • P - phosphating,
  • PO - phosphating and oiling,
  • U - untreated

Designation of the coating appearance for Z and ZF coatings on flat products:

  • N - normal zinc spangle
  • M - small zinc spangle,
  • R - zinc-iron coating of standard quality (matt grey)

Surface quality designations for Z and ZF coatings:

  • A - normal surface,
  • B - improved surface (by skin-pass rolling),
  • C - highest-quality surface (also after skin-pass rolling).

Galvanic corrosion and corrosion in water

Connecting zinc-coated steel to copper or brass in the presence of water or in a polluted atmosphere can lead to galvanic corrosion.

The behaviour of galvanized steel in aqueous solutions is affected by the following factors:

  • pH - the corrosion rate is low at pH values between 6 and 12. Lower or higher pH values accelerate corrosion.
  • water hardness - the harder the water, the slower the corrosion.
  • temperature above 60°C significantly accelerates corrosion.
  • chloride content can cause rapid corrosion.

Hot-dip zinc coating (Zn)

During the hot-dip galvanizing of steel, several intermetallic phases with different chemical compositions, crystal structures and properties are formed. The thickness of these layers depends on the chemical composition and temperature of the bath, immersion rate, cooling conditions and any subsequent reheating. The following is a list of these layers and their properties, starting with the outermost:

  • eta layer η, almost 100% zinc, melting point 419°C, hexagonal crystal structure, 70-72 HV, soft and ductile;
  • zeta layer ζ, FeZn13 (~95% zinc), melting point 530°C, monoclinic crystal structure, 175-185 HV, hard and brittle;
  • delta layer δ, FeZn7 (~90% zinc), melting range 530-670°C, hexagonal crystal structure, 240-300 HV, ductile;
  • gamma layer γ, Fe3Zn10 (~73% zinc), melting range 670-780°C, cubic crystal structure, very brittle;
  • alpha layer α, almost pure iron, melting point 1510°C, cubic crystal structure, soft and ductile;

The intermetallic phases bond the steel substrate to the Zn coating. A thick gamma layer can result in poor adhesion between the coating and the substrate. Adding 0.1-0.25% Al limits the formation of this layer. For applications requiring a non-shiny surface, i.e. a surface without visible spangles, a galvanizing bath with a lead content below 0.15% is used. By contrast, adding antimony produces a shiny, spangled surface. Zinc coatings have self-lubricating properties, which is beneficial during forming. The coating retains its colour at temperatures up to 230°C.

Crystalline surface of a hot-dip galvanized steel, known as "spangle"

Properties of hot-dip coatings applied to strip according to PN-EN 10326 and PN-EN 10327 (the minimum coating mass refers to both sides):

Z100:

  • Minimum coating mass: 100 g⋅m-2 
  • Coating thickness per side: 7 μm
  • Coating density: 7.1 Mg⋅m-3 

Z140:

  • Minimum coating mass: 140 g⋅m-2 
  • Coating thickness per side: 10 μm
  • Coating density: 7.1 Mg⋅m-3 

Z200:

  • Minimum coating mass: 200 g⋅m-2 
  • Coating thickness per side: 14 μm
  • Coating density: 7.1 Mg⋅m-3 

Z225:

  • Minimum coating mass: 225 g⋅m-2 
  • Coating thickness per side: 16 μm
  • Coating density: 7.1 Mg⋅m-3 

Z275:

  • Minimum coating mass: 275 g⋅m-2 
  • Coating thickness per side: 20 μm
  • Coating density: 7.1 Mg⋅m-3 

Z350:

  • Minimum coating mass: 350 g⋅m-2 
  • Coating thickness per side: 25 μm
  • Coating density: 7.1 Mg⋅m-3 

Z450:

  • Minimum coating mass: 450 g⋅m-2 
  • Coating thickness per side: 32 μm
  • Coating density: 7.1 Mg⋅m-3 

Z600:

  • Minimum coating mass: 600 g⋅m-2 
  • Coating thickness per side: 42 μm
  • Coating density: 7.1 Mg⋅m-3 

Hot-dip zinc-iron coating (Zn-Fe)

Compared with Zn coatings, Zn-Fe coatings offer better weldability and resistance spot welding performance, while providing similar corrosion resistance and paint adhesion. They are most commonly used in the automotive industry. The coating process is similar to that used for Zn coatings, except that after leaving the zinc bath, the strip is inductively heated to 500-550°C. This causes the multiple layers normally formed in a Zn coating to transform into a uniform delta layer δ (described above). The resulting coating has a matt grey appearance with no visible spangle.

Properties of hot-dip coatings applied to strip according to PN-EN 10326 and PN-EN 10327 (the minimum coating mass refers to both sides):

ZF100:

  • Minimum coating mass: 100 g⋅m-2 
  • Coating thickness per side: 7 μm
  • Coating density: 7.1 Mg⋅m-3 

ZF120:

  • Minimum coating mass: 120 g⋅m-2 
  • Coating thickness per side: 8 μm
  • Coating density: 7.1 Mg⋅m-3 

ZF140:

  • Minimum coating mass: 140 g⋅m-2 
  • Coating thickness per side: 10 μm
  • Coating density: 7.1 Mg⋅m-3 

Hot-dip aluminium coating (Al)

Compared with a Zn coating, an aluminium coating provides significantly better corrosion resistance, with a corrosion rate that is 4-5 times lower. It also offers excellent resistance to high-temperature corrosion, remaining stable at temperatures of up to 500°C in the presence of exhaust gases without any change in appearance. Under certain conditions, the coating can withstand temperatures of up to 1150°C without any visible change. Aluminium also just nice to look at. It is therefore widely used for coating automotive exhaust components, such as mufflers.

Hot-dip aluminium-silicon coating (Al-Si)

This coating is similar to a pure aluminium coating, but the addition of silicon prevents the formation of a thick Fe-Al intermetallic layer. As a result, the coating has good adhesion to the steel substrate and the coated strip retains good formability. 

Properties of hot-dip coatings applied to strip according to PN-EN 10326 and PN-EN 10327 (the minimum coating mass refers to both sides):

AS060:

  • Minimum coating mass: 60 g⋅m-2 
  • Coating thickness per side: 8 μm
  • Coating density: 3.0 Mg⋅m-3 

AS080:

  • Minimum coating mass: 80 g⋅m-2 
  • Coating thickness per side: 14 μm
  • Coating density: 3.0 Mg⋅m-3 

AS100:

  • Minimum coating mass: 100 g⋅m-2 
  • Coating thickness per side: 17 μm
  • Coating density: 3.0 Mg⋅m-3 

AS120:

  • Minimum coating mass: 120 g⋅m-2 
  • Coating thickness per side: 20 μm
  • Coating density: 3.0 Mg⋅m-3 

AS150:

  • Minimum coating mass: 150 g⋅m-2 
  • Coating thickness per side: 25 μm
  • Coating density: 3.0 Mg⋅m-3 

Hot-dip aluminium-zinc coating (Al-Zn)

The coating consists of 55% aluminium, 1.6% silicon and the balance zinc. It is applied using a process similar to hot-dip galvanizing. It provides 2 to 4 times better corrosion resistance than a conventional zinc coating because zinc and aluminium corrode in separate phases. During the initial period of service, the Zn-rich phase corrodes preferentially, while the resulting corrosion products inhibit further oxidation. Zinc also provides sacrificial protection to exposed cut edges and damaged areas of the coating because it has a lower electrochemical potential than iron. Once the Zn-rich phase is consumed, corrosion protection is provided by the Al-rich phase. Unlike a conventional zinc coating, this coating does not have self-lubricating properties, so a suitable lubricant should be used when forming products from coated sheet. It also has better high-temperature resistance than a conventional zinc coating.

Appearance - bright, attractive silver appearance. The coating retains its colour at temperatures up to 310°C.

Properties of hot-dip coatings applied to strip according to PN-EN 10326 and PN-EN 10327 (the minimum coating mass refers to both sides):

AZ100:

  • Minimum coating mass: 100 g⋅m-2 
  • Coating thickness per side: 13 μm
  • Coating density: 3.8 Mg⋅m-3 

AZ150:

  • Minimum coating mass: 150 g⋅m-2 
  • Coating thickness per side: 20 μm
  • Coating density: 3.8 Mg⋅m-3 

AZ185:

  • Minimum coating mass: 185 g⋅m-2 
  • Coating thickness per side: 25 μm
  • Coating density: 3.8 Mg⋅m-3 

Hot-dip zinc-aluminium coating (Zn-Al)

The coating consists of 95% Zn with a 5% Al addition. It provides better corrosion protection than a pure Zn coating while offering similarly good formability. 

Properties of hot-dip coatings applied to strip according to PN-EN 10326 and PN-EN 10327 (the minimum coating mass refers to both sides):

ZA095:

  • Minimum coating mass: 95 g⋅m-2 
  • Coating thickness per side: 7 μm
  • Coating density: 6.9 Mg⋅m-3 

ZA130:

  • Minimum coating mass: 130 g⋅m-2 
  • Coating thickness per side: 10 μm
  • Coating density: 6.9 Mg⋅m-3 

ZA185:

  • Minimum coating mass: 185 g⋅m-2 
  • Coating thickness per side: 14 μm
  • Coating density: 6.9 Mg⋅m-3

ZA200:

  • Minimum coating mass: 200 g⋅m-2 
  • Coating thickness per side: 15 μm
  • Coating density: 6.9 Mg⋅m-3 

ZA255:

  • Minimum coating mass: 255 g⋅m-2 
  • Coating thickness per side: 20 μm
  • Coating density: 6.9 Mg⋅m-3 

ZA300:

  • Minimum coating mass: 300 g⋅m-2 
  • Coating thickness per side: 23 μm
  • Coating density: 6.9 Mg⋅m-3 

Hot-dip lead-tin coating (Pb-Sn)

The coating bath contains 3-15% tin (Sn), with lead (Pb) making up the balance. In practice, tin does not dissolve in lead, so the coating consists primarily of a lead matrix with tin present as discrete inclusions. The coating provides good corrosion resistance as well as very good weldability, solderability and deep drawability, as it acts as a lubricant during forming. Steel strip with this type of coating is used for fuel tanks and fuel lines. The coating is not shiny and looks rather dull.

Hot-dip phosphate coating

The coating consists of crystalline phosphate with a thickness of 3-50 μm and is formed by immersing the strip in a solution of zinc, manganese or iron phosphates with suitable additives. The coating has excellent adhesion to the substrate. However, because it is porous, it does not provide long-term corrosion protection, nor is this its primary purpose. It readily absorbs lubricants, improves the adhesion of paints and coatings, and increases resistance to abrasive wear. It is therefore used as a primer layer for paints and coatings on unalloyed, uncoated steel strip.

Zinc electrogalvanization (Zn)

The plating solution consists mainly of zinc sulphate, while the anodes are made of lead. After zinc plating, the strip passes through a chromate bath, where a passive layer is formed. The coating is very thin, and its application does not cause ageing. As a result, it provides excellent formability, although it decreases significantly as the coating thickness increases. This type of coating is widely applied to low-carbon steels intended for cold forming and used in the furniture, packaging, automotive and household appliance industries.

Properties of coatings applied to strip according to PN-EN 10152 :

ZE18:

  • Minimum coating mass: 18 g⋅m-2 
  • Coating thickness per side: 2.5 μm

ZE36:

  • Minimum coating mass: 36 g⋅m-2 
  • Coating thickness per side: 5.0 μm

ZE54:

  • Minimum coating mass: 54 g⋅m-2 
  • Coating thickness per side: 7.5 μm

ZE72:

  • Minimum coating mass: 72 g⋅m-2 
  • Coating thickness per side: 10 μm

Zinc-nickel electrogalvanization (Zn-Ni)

A zinc coating containing 10.5-13% nickel, providing better corrosion resistance than a pure zinc coating of the same thickness.

Properties of coatings according to PN-EN 10271:

ZN15:

  • Minimum coating mass: 15 g⋅m-2 
  • Coating thickness per side: 2 μm

ZN44:

  • Minimum coating mass: 44 g⋅m-2 
  • Coating thickness per side: 6 μm

Zinc-iron electrogalvanization (Zn-Fe)

A zinc coating containing 8-20% iron, providing better paint adhesion and corrosion resistance than a pure zinc coating of the same thickness. These coatings are used in the automotive industry. Applying this type of coating requires precise control of the electrolyte temperature and chemical composition.

Coating properties:

ZnFe50:

  • Minimum coating mass: 50 g⋅m-2 
  • Coating thickness per side: 7 μm

Post author

Piotr Sompoliński

CSO Virgamet

Featured Posts

Need help? Contact us!

Call or send a message, and our representative
will contact you within 24 hours!

We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie preferences
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.