65G, 65Mn4, 66Mn4, 1.1240, 1.1260 - Manganese spring alloy structural steel according to PN-74/H-84032

 

Standard Steel Grade
Chemical Composition %
C: Mn: Si: P: S: Cr: Ni: Al: Cu:
PN 65G
0.6 - 0.7 0.90 - 1.20 0.15 - 0.40 <0.04 <0.04 <0.3 <0.3 - <0.25
DIN 66Mn4 - 66 Mn 4 - 1.1260
0.60 - 0.71 0.85 - 1.15 0.15 - 0.30 <0.035 <0.035 - - - -
DIN 65Mn4 - 65 Mn 4 - 1.1240
0.60 - 0.70 0.90 - 1.20 0.25 - 0.50 <0.035 <0.035 - - - -
ISO 56Mn4 - 56 Mn 4 - 1.1233
0.52 - 0.60 0.90 - 1.20 <0.40 <0.025 <0.03 - - <0.05 <0.3
GOST 65G - 65Г
0.62 - 0.70 0.90 - 1.20 0.17 - 0.37 <0.035 <0.035 <0.25 <0.25 - -
GOST 65GA - 65ГА
0.65 - 0.70 0.7 - 1.0 0.15 - 0.30 <0.025 <0.025 <0.15 <0.2 <0.08 <0.2
STAS 65MN10 - 65 Mn 10
0.62 - 0.70 0.90 - 1.20 0.17 - 0.37 <0.035 <0.035 <0.3 <0.3 - <0.3
ČSN / STN ČSN 13 180 - ČSN 13180
0.70 - 0.80 0.90 - 1.20 0.15 - 0.35 <0.035 <0.04 <0.3 <0.4 - <0.3
SAE AISI C1062 - 1062
0.54 - 0.65 0.85 - 1.15 - <0.04 <0.05 - - - -
UNS AISI 1066 - AISI 1566
0.60 - 0.71 0.85 - 1.15 - <0.04 <0.05 - - - -

 

65G steel - specification and application

65G - Steel for leaf springs and springs with low hardenability requiring increased resistance to abrasion for rings, valve springs, flat, coils and spring washers with small cross-sections and loads. Steel for hardening in oil insensitive to temper brittleness. Steel does not show resistance to corrosive environments.


Mechanical and physical properties of 65G steel

  • Tensile strength, Rm ≥ 980 MPa
  • The yield strength, Re ≥ 780 MPa
  • Contraction, Z ≥ 30%
  • Elongation, A ≥ 8%
  • Hardness after softening ≤ 241 HB
  • Hardness in raw condition: ≤ 262 HB
  • Hardness after hardening and tempering in a temp. of 380-520℃ = 42 - 47 HRC
  • Hardness after hardening and tempering in 400 - 550 ℃ = 310 - 350 HB
  • Density ρ = ~ 7,83 kg / dm3
  • Thermal conductivity λ20 ℃ = ~ 46,2 W ⋅ m-1 K-1
  • Thermal capacity cp20-100 ℃ = ~ 481 J ⋅ kg-1 K-1
  • Linear expansion coefficient α20-100℃ = ~11,35 10-6 K-1

 


In the described grade, the company provides:

 


The list of equivalents and other designations of 65G steel:

66Mn4, 66 Mn 4, 1.1260, 65Mn4, 65 Mn 4, 1.1240, 56Mn4, 56 Mn 4, 1.1233, 65Г, 65GA, 65ГА, 65MN10, 65 Mn 10, ČSN 13 180, ČSN 13180, AISI C1062, 1062, AISI 1066, AISI 1566


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.