45HN, 40ChN, 40KhN - alloy structural steel for thermal improvement in accordance with PN-89/H-84030/04 and PN-72/H-84030.

 

StandardsSteel Grades
Chemical Composition %
C:Mn:Si:P:S:Cr:Mo:Ni:V:Ti:Cu:N:W:
PN45HN
0.41 - 0.490.5 - 0.80.17 - 0.37<0.035<0.0350.45 - 0.75-1.0 - 1.4-----
GOST45ChN - 45KhN - 45ХН
0.41 - 0.490.5 - 0.80.17 - 0.37<0.035<0.0350.45 - 0.75<0.151.0 - 1.4<0.05<0.03<0.30<0.008<0.2
GOST40ChN - 40KhN - 40ХН
0.36 - 0.440.5 - 0.8<0.20<0.035<0.0350.45 - 0.75<0.151.0 - 1.4<0.05<0.03<0.30<0.008<0.2
GB/T45CrNi - A40452 - A 40452
0.42 - 0.490.5 - 0.80.17 - 0.37<0.035<0.0350.45 - 0.75<0.151.0 - 1.4--<0.30--
GOST40ChN-Sh - 40KhN-Sh - 40ХН-ш
0.36 - 0.440.5 - 0.80.17 - 0.37<0.025<0.0150.45 - 0.75<0.151.0 - 1.4<0.05<0.03<0.25<0.008<0.2
JISSNC 236 - SNC 1 - SNC236 - SNC1
0.32 - 0.400.5 - 0.80.15 - 0.35<0.030<0.0300.50 - 0.90-1.0 - 1.5--<0.30--
БДС45ChN - 45KhN - 45ХН
0.41 - 0.490.5 - 0.80.17 - 0.37<0.035<0.0350.45 - 0.75<0.151.0 - 1.4<0.05<0.03<0.30-<0.2

 

Steel 45HN - Specification and application

Structural alloy steel with medium hardenability for thermal improvement, surface hardening - flame and inductive hardening, high strength, ductility and impact and abrasion resistance.

Used for parts of machines, motors, and motor vehicles which, due to their dimensions, cannot be carburized. The soaking of products in a cyanide salt bath increases the resistance to abrasion. The 45HN grade is also suitable for surface hardening after thermal improvement.

In addition, it has an improved surface abrasion resistance which it acquires during heating in saline bath containing cyanide. Moreover, the good feature of the 45HN grade is the resistance to deformation during hardening.

45HN steel is hard to weld, and treatment in exceptional cases should be done after softening. Used as steel for machine shafts, pinion cogwheels, toothed rims, screws, forged and folded shafts, piston rods for steam engines, hammers and pumps.


Mechanical properties of the 45HN grade

Mechanical properties
Tensile strengthRm> 1030 MPa
Yield pointRe> 835 MPa
Notch toughnessKCU> 56 J
ContractionZ> 45 %
ElongationA> 10 %
Densityρ~7,83 kg/dm3
Hardness in softened stateHB< 207 HB

 

PropertiesDimensions
<16mm16 - 40mm40 - 100mm100 - 160mm
Tensile strengthRm1080 - 1230 MPa980 - 1130 MPa830 - 980 MPa740 - 880 MPa
Yield pointRe> 880 MPa> 780 MPa> 690 MPa> 540 MPa
Notch toughnessKCU-> 40 J> 40 J-
ContractionZ> 40 %> 45 %> 45 %> 45 %
ElongationA> 9 %> 10 %> 12 %> 13 %

 


Heat treatment of 45HN steel

- For large dimensions 45HN steel is hardened in oil

- Tempering in 45HN water is done in water to avoid temper brittleness

Heat treatment typeCooling typeTemperatures
Normalizing annealingin calm air840 - 880℃
Softening annealingslow cooling680 - 720℃
Hardeningin water810 - 840℃
w oleju820 - 850℃
Temperingin water550 - 650℃
in air550 - 650℃

 


Welding, joining and cutting of 45HN steel

45HN steel products can be arc plasma, oxyacetylene, and propane-butane oxygen cut. Before cutting steel needs to be heated to 250 - 300 ℃. After cutting, the steel should be cooled in the air.

45HN can be frictionally, resistively or electrically welded in a softened and heat-treated state, making after the process a suitable heat treatment to maintain stable material parameters.

As mentioned above, 45HN steel does not belong to easily weldable grades. The treatment should be performed only in exceptional circumstances in the softened state of delivery of the material. Steel with a much larger dimensions requires interoperable relacing annealing.

Steel can be arc-welded with coated electrodes or in CO 2 casing with pre-heating of the material to appropriate temperatures. When the welding procedure is completed before the material has cooled down, the joints should be subjected to softening annealing.

If the conditions do not allow for treatment, the steel should be covered with mats or cooled in the hot sand.

Below the temperature table for preheating the material before welding.

Temperatures of soaking of 45HN material
Dimensions< 15mm15 - 25mm25 - 50mm
Temperatures150 - 250℃200 - 300℃250 - 350℃

 


In the 45HN grade the company delivers:

 


List of equivalents and other determinations of 45HN steel:

45ChN, 45KhN, 45ХН, 40ChN, 40KhN, 40ХН, 45CrNi, A40452, A 40452, 40ChN-Sh, 40KhN-Sh, 40ХН-ш, SNC 236, SNC 1, SNC236, SNC1, 45ChN, 45KhN, 45ХН


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.