40CrMoV4-6, 1.7711 - Structural boiler steel for operation at elevated temperatures according to EN 10269.

Standard Steel Grade
Chemical composition %
C: Mn: Si: P: S: Cr: Mo: V: Al:
EN 40CrMoV4-6 - 1.7711
0.36 - 0.44 0.45 - 0.55 <0.4 <0.025 <0.030 0.9 - 1.2 0.50 - 0.65 0.25 - 0.35 <0.015
ASTM SA193 / A193 gr. B16 - SA194 / A194 gr. 16
0.36 - 0.47 0.45 - 0.70 0.15 - 0.35 <0.035 <0.040 0.80 - 1.15 0.50 - 0.65 0.25 - 0.35 <0.015
UNS UNS K14072
0.36 - 0.44 0.45 - 0.70 0.15 - 0.35 <0.040 <0.040 0.80 - 1.15 0.50 - 0.65 0.25 - 0.35 <0.015
IS 40CrMoVH
0.36 - 0.44 0.45 - 0.85 0.10 - 0.35 <0.030 <0.030 0.90 - 1.20 0.55 - 0.75 0.25 - 0.35 -

 


40CrMoV4-6, 1.7711 - specification and application

High-temperature structural steel for bolts, nuts, motor and machine components such as crankshafts, axles, spindles and gears.

 


Mechanical properties of 40CrMoV4-6, 1.7711 +QT:

  • Tensile strength, Rm 850-1000 MPa
  • Yield strength, Rp0,2: >640 MPa
  • Elongation, A: >14%
  • Necking, Z: >45%
  • Impact strength, KV: > 25J
  • Hardness: 250-300 HB

 


Mechanical properties at elevated temperatures

Temperatures (℃) 50 100 150 200 250 300 350 400 450 500 550 600
Yield strength, Rp0,2 (MPa) >630 >610 >590 >575 >550 >540 >525 >507 >480 >430 >365 >268

 


Heat treatment of 40CrMoV4-6, 1.7711 steel:

  • Annealing at a temperature of 680 - 730C
  • Normalization at a temperature of 880 - 900C
  • Annealing at a temperature of 830C
  • Annealing at a temperature of 900 - 930C
  • Normalization at a temperature of 650 - 720C
  • Stress relief annealing after hardening at a temperature of 200C
  • Stress relief annealing at a temperature 50C lower than tempering

 


In the above mentioned grades the company delivers:

 


Other designations of the grade:

40CrMoV4-6, 40CrMoV4-7, 1.7711, A193 grade B16, A194 grade 16, BS670-860


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.