Structural alloy steel 39NiCrMo3, 1.6510, 38NiCrMo4, 38NCD4 for heat treatment for heavy-duty parts of machines, engines and aircrafts according to EN 10083-1.

 

Standards Steel Grades
Chemical Composition %
C: Mn: Si: P: S: Cr: Mo: Ni:
PN 38HNM
0.34 - 0.43 0.50 - 0.80 0.17 - 0.37 <0.035 <0.035 0.60 - 0.90 0.15 - 0.25 0.70 - 1.00
EN 39NiCrMo3 - 1.6510
0.35 - 0.43 0.50 - 0.80 <0.40 <0.025 <0.035 0.60 - 1.00 0.15 - 0.25 0.70 - 1.00
GOST 39ChNM - 39KhNM - 39ХНМ
0.35 - 0.43 0.50 - 0.80 <0.40 <0.025 <0.035 0.60 - 1.00 0.15 - 0.25 0.70 - 1.00
UNI 38NiCrMo4KB - 38 NiCrMo 4 KB
0.35 - 0.43 0.50 - 0.80 0.15 - 0.40 <0.035 <0.035 0.70 - 1.00 0.15 - 0.30 0.70 - 1.00
UNE F-128 - A-128
0.30 - 0.40 0.55 - 0.85 0.10 - 0.35 <0.040 <0.040 0.80 - 1.20 0.20 - 0.40 0.80 - 1.20
MSZ NCMo4
0.36 - 0.43 0.50 - 0.80 0.15 - 0.40 <0.035 <0.035 0.60 - 0.90 0.15 - 0.30 0.70 - 1.00
UNI 38NCD4 - 38 NCD 4
0.35 - 0.43 0.50 - 0.80 0.15 - 0.35 <0.035 <0.035 0.60 - 1.00 0.15 - 0.25 0.70 - 1.00
JUS Č.5430 - Č5430
0.32 - 0.40 0.50 - 0.80 0.15 - 0.40 <0.035 <0.035 0.90 - 1.20 0.15 - 0.30 0.90 - 1.20

 

Steel 39NiCrMo3, 1.6510, 38HNM - description and specification

Steel with high hardening capacity and good toughness, which allows to achieve optimum mechanical properties with dimensions up to approx. 80mm. Used on heavy-duty machinery parts, automotive accessories and other motor vehicles, including engine parts.

38HNM steel is hardened in oil and water, and its weldability is quite limited. Designed for heavy-duty rotary shafts, steam turbine rings, compressor parts, propeller hub, engine pump parts, steam turbine wheels, crankshaft, press parts and shafts for steam turbines.


General mechanical properties of 39NiCrMo3, 1.6510 steel

Properties of 39NiCrMo3 steel
Yield point Re < 740 MPa
Tensile strength Rm > 880 MPa
Contraction Z -
Notch toughness KU2 > 80 J
Elongation A > 12 %
Density ρ ~7,85 kg/dm3
Hardness in softened state HB < 229 HB

 


Mechanical properties of 39NiCrMo3, 1.6510 steel for individual dimensions

Properties Dimensions
<16mm 16 - 40mm 40 - 100mm 100 - 160mm 160 - 250mm
Yield point Re >755 MPa >735MPa > 685 MPa > 635 MPa > 540 MPa
Tensile strength Rm 980 - 1180 MPa 930 - 1130 MPa 880 - 1080 MPa 830 - 980 MPa 740 - 880 MPa
Contraction Z >40% >40% >45% >50% >50%
Notch toughness KU2 - >35J >40J >40J >40J
Elongation A >11 % >11 % >12 % >12 % >13 %

 


Heat treatment of 39NiCrMo3, 1.6510 steel - processes, cooling and temperature

Heat treatment - processes
Process Cooling type Temperature
Normalizing annealing in calm air 830 - 860℃
Softening annealing slow 650 - 700℃
Hardening in oil 830 - 850℃
in water
Tempering min. 1h in air 550 - 650℃

 


In the 38HNM grade the company provides:

 


List of other designations and equivalents of 38HNM steel:

39NiCrMo4, 1.6510, 39ChNM, 39KhNM, 39ХНМ, 38NiCrMo4KB, 39NiCrMoS3, 39NiCrMoS3HH, 39NiCrMo3Pb, 38 NiCrMo 4 KB, F-128, A-128, NCMo4, 38NCD4, 38 NCD 4, Č.5430, Č5430.


We use cookies
In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy. You can specify the detailed configuration by clicking the button below "Settings".
Cookie settings
We use cookies

In order to properly operate the Website and for statistical purposes, and if you consent, also to personalize advertising, remarketing and retargeting. If you want to learn more, read on privacy and cookies policy.

More information

If you have any questions about our cookie policy, please ask contact.